JPH04238670A - 裏波ビード溶接方法 - Google Patents
裏波ビード溶接方法Info
- Publication number
- JPH04238670A JPH04238670A JP2418825A JP41882590A JPH04238670A JP H04238670 A JPH04238670 A JP H04238670A JP 2418825 A JP2418825 A JP 2418825A JP 41882590 A JP41882590 A JP 41882590A JP H04238670 A JPH04238670 A JP H04238670A
- Authority
- JP
- Japan
- Prior art keywords
- welding
- bead
- backing
- uranami
- welding method
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
め要約のデータは記録されません。
Description
【0001】
【産業上の利用分野】この発明は裏波ビード溶接方法に
関するものである。
関するものである。
【0002】
【従来の技術】裏当材を全く使用しない裏波ビード溶接
方法は、その溶接裏面側に切欠等が存在しないことから
、疲労強度をはじめとする継手性能が優れている反面、
健全な裏ビードを形成するためには、厳しい部品加工精
度、組立精度及び溶接条件管理が必要とされる。
方法は、その溶接裏面側に切欠等が存在しないことから
、疲労強度をはじめとする継手性能が優れている反面、
健全な裏ビードを形成するためには、厳しい部品加工精
度、組立精度及び溶接条件管理が必要とされる。
【0003】その一方、裏当材を使用する場合には、上
記のような厳しい精度等は要求されないものの、裏当材
の存在に起因する残留スリットが原因で継手性能に難点
がある。また裏当材の設置には、ある程度の精度が必要
であるし、またそれに応じた手数を要する。
記のような厳しい精度等は要求されないものの、裏当材
の存在に起因する残留スリットが原因で継手性能に難点
がある。また裏当材の設置には、ある程度の精度が必要
であるし、またそれに応じた手数を要する。
【0004】
【発明が解決しようとする課題】そこでこの発明は、従
来の裏波ビード溶接方法のように厳しい精度等を必要と
せず、しかも従来の裏波溶接と略同様に残留スリットの
存しない健全な裏ビードを形成することが可能な裏波ビ
ード溶接方法を提供することを、課題とする。
来の裏波ビード溶接方法のように厳しい精度等を必要と
せず、しかも従来の裏波溶接と略同様に残留スリットの
存しない健全な裏ビードを形成することが可能な裏波ビ
ード溶接方法を提供することを、課題とする。
【0005】
【課題を解決するための手段】本発明は、一方の母材の
溶接部裏面側に消耗式アーク溶接法によるビードオンプ
レート溶接によって裏当ビード部を形成し、他方の母材
の開先裏面側の端部を上記裏当ビード部に当接させるか
、あるいはその近傍に配置し、次いで表側から溶接を行
うことで上記裏当ビード部と他方の開先裏面側との間に
裏波ビードを形成する点を主要な特徴とするもので、こ
れにより上記課題を解決した。
溶接部裏面側に消耗式アーク溶接法によるビードオンプ
レート溶接によって裏当ビード部を形成し、他方の母材
の開先裏面側の端部を上記裏当ビード部に当接させるか
、あるいはその近傍に配置し、次いで表側から溶接を行
うことで上記裏当ビード部と他方の開先裏面側との間に
裏波ビードを形成する点を主要な特徴とするもので、こ
れにより上記課題を解決した。
【0006】
【作用】上記裏波ビード溶接方法においては、裏当ビー
ド部と他方の開先裏面側との間に裏波ビードが形成され
るが、裏当ビード部は、一方の母材と一体と見做せるの
で、一方の母材、裏当ビード部、裏波ビード、他方の母
材に至る経路間にスリットが残留することはない。また
溶接に際し、裏当ビード部は、裏波ビードの溶落ちを防
止する裏当材としても機能することになるので、裏波ビ
ードの形成が容易になる。
ド部と他方の開先裏面側との間に裏波ビードが形成され
るが、裏当ビード部は、一方の母材と一体と見做せるの
で、一方の母材、裏当ビード部、裏波ビード、他方の母
材に至る経路間にスリットが残留することはない。また
溶接に際し、裏当ビード部は、裏波ビードの溶落ちを防
止する裏当材としても機能することになるので、裏波ビ
ードの形成が容易になる。
【0007】
【実施例】まず図1のように、一方の母材1の溶接部裏
面側に、消耗式アーク溶接法によるビードオンプレート
溶接によって裏当ビード部2を形成しておく。溶接とし
ては、MIG溶接、炭酸ガス溶接、被覆アーク溶接等の
任意のものを選択し得る。また溶接姿勢としては、母材
1を水平に配置した下向き溶接で行うのが好ましいが、
もちろんこれに限られる訳でなはい。
面側に、消耗式アーク溶接法によるビードオンプレート
溶接によって裏当ビード部2を形成しておく。溶接とし
ては、MIG溶接、炭酸ガス溶接、被覆アーク溶接等の
任意のものを選択し得る。また溶接姿勢としては、母材
1を水平に配置した下向き溶接で行うのが好ましいが、
もちろんこれに限られる訳でなはい。
【0008】次いで他方の母材3の開先裏面側の端部を
、図1のように上記裏波ビード部2のやや上側の位置に
配置し、この状態で表面側からアーク溶接を行う。そう
すると図2に示すように、裏波ビード部2と他方の母材
3の裏面側との間に、裏波ビード4が形成される。
、図1のように上記裏波ビード部2のやや上側の位置に
配置し、この状態で表面側からアーク溶接を行う。そう
すると図2に示すように、裏波ビード部2と他方の母材
3の裏面側との間に、裏波ビード4が形成される。
【0009】上記裏波ビード溶接方法によれば、裏波ビ
ードに際して、裏当ビード部2が裏波ビード4の溶落ち
を防止する裏当材として機能するので、ルートギャップ
に多少の変動があってもよく、そのため部品加工精度、
組立精度及び溶接条件管理等に高水準のものが要求され
ることはない。また溶接裏面側においては、一方の母材
1、裏当ビード部2、裏波ビード4、他方の母材3に至
る経路に、従来の裏当材を用いるような場合に生じてい
たスリットが残留することもない。
ードに際して、裏当ビード部2が裏波ビード4の溶落ち
を防止する裏当材として機能するので、ルートギャップ
に多少の変動があってもよく、そのため部品加工精度、
組立精度及び溶接条件管理等に高水準のものが要求され
ることはない。また溶接裏面側においては、一方の母材
1、裏当ビード部2、裏波ビード4、他方の母材3に至
る経路に、従来の裏当材を用いるような場合に生じてい
たスリットが残留することもない。
【0010】図3の実施例は、次のような条件にて溶接
を行ったものである。すなわち裏当ビード部は、溶接電
圧20V、溶接電流150A、溶接速度36cm/分の
炭酸ガスアーク溶接法にて形成した。また他方の母材と
して板厚12mm、開先角度45度のものを使用してい
る。裏波ビード溶接条件は、溶接電圧26V、溶接電流
250A、溶接速度35cm/分の炭酸ガスアーク溶接
法により行っている。
を行ったものである。すなわち裏当ビード部は、溶接電
圧20V、溶接電流150A、溶接速度36cm/分の
炭酸ガスアーク溶接法にて形成した。また他方の母材と
して板厚12mm、開先角度45度のものを使用してい
る。裏波ビード溶接条件は、溶接電圧26V、溶接電流
250A、溶接速度35cm/分の炭酸ガスアーク溶接
法により行っている。
【0011】上記溶接法によれば、図3のように溶接欠
陥のない、良好な溶接継手を得ることができる。
陥のない、良好な溶接継手を得ることができる。
【0012】なお上記裏波ビード溶接における溶接姿勢
は、下向きに限らず、どのような姿勢であってもよいし
、また溶接層数は単層、多層のいずれで実施してもよい
。さらに上記溶接方法を適用し得る溶接継手形状も、図
1〜図3のものに限られず、図4、図5に示すものをは
じめとする種々形状に適用が可能である。
は、下向きに限らず、どのような姿勢であってもよいし
、また溶接層数は単層、多層のいずれで実施してもよい
。さらに上記溶接方法を適用し得る溶接継手形状も、図
1〜図3のものに限られず、図4、図5に示すものをは
じめとする種々形状に適用が可能である。
【0013】
【発明の効果】この発明の裏波ビード溶接方法によれば
、一方の母材に一体形成された裏波ビードに裏当材とし
ての機能を持たせながら裏波溶接を行うようにしてある
ので、残留スリットの存しない良好な裏波溶接を行いな
がらも、裏波ビード形成部でのギャップ裕度が従来より
も大となる。そのため部品加工精度、組立精度に従来の
ような高い精度が要求されず、また溶接可能条件の裕度
が大となり、溶接施工能率を向上し得る。
、一方の母材に一体形成された裏波ビードに裏当材とし
ての機能を持たせながら裏波溶接を行うようにしてある
ので、残留スリットの存しない良好な裏波溶接を行いな
がらも、裏波ビード形成部でのギャップ裕度が従来より
も大となる。そのため部品加工精度、組立精度に従来の
ような高い精度が要求されず、また溶接可能条件の裕度
が大となり、溶接施工能率を向上し得る。
【0014】しかも裏当材を使用する場合、複雑形状の
構造物では、該複雑な形状に沿って正確に裏当材を成形
、配置する必要があるが、この発明方法ではビードオン
プレート溶接を行うだけでよいことから、溶接施工能率
はこの点においても向上することになる。
構造物では、該複雑な形状に沿って正確に裏当材を成形
、配置する必要があるが、この発明方法ではビードオン
プレート溶接を行うだけでよいことから、溶接施工能率
はこの点においても向上することになる。
【図面の簡単な説明】
【図1】この発明の裏波ビード溶接方法の一実施例の溶
接前の状態の説明図である。
接前の状態の説明図である。
【図2】本発明方法の一実施例の溶接後の状態の説明図
である。
である。
【図3】本発明により得られた溶接継手部の金属組織を
示す図である。
示す図である。
【図4】本発明方法を適用し得る他の継手形状の説明図
である。
である。
【図5】本発明方法を適用し得るさらに他の継手形状の
説明図である。
説明図である。
1 母材
2 裏当ビード部
3 母材
4 裏波ビード
Claims (1)
- 【請求項1】 一方の母材の溶接部裏面側に消耗式ア
ーク溶接法によるビードオンプレート溶接によって裏当
ビード部を形成し、他方の母材の開先裏面側の端部を上
記裏当ビード部に当接させるか、あるいはその近傍に配
置し、次いで表側から溶接を行うことで上記裏当ビード
部と他方の開先裏面側との間に裏波ビードを形成するこ
とを特徴とする裏波ビード溶接方法。