JPH0446942A - Preparation of phenol resin foam - Google Patents
Preparation of phenol resin foamInfo
- Publication number
- JPH0446942A JPH0446942A JP15643890A JP15643890A JPH0446942A JP H0446942 A JPH0446942 A JP H0446942A JP 15643890 A JP15643890 A JP 15643890A JP 15643890 A JP15643890 A JP 15643890A JP H0446942 A JPH0446942 A JP H0446942A
- Authority
- JP
- Japan
- Prior art keywords
- blowing agent
- phenolic resin
- foam
- sulfonylhydrazine
- foaming
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
Description
【発明の詳細な説明】
[産業上の利用分野]
本発明は建材用として壁材、天井材、また家具等の材料
として有用な耐熱性、断熱性、難燃性、耐水性を有し1
機械的強度に優れたフェノール樹脂発泡体の製造法に関
する。[Detailed Description of the Invention] [Industrial Application Field] The present invention has heat resistance, heat insulation, flame retardancy, and water resistance and is useful as a building material for wall materials, ceiling materials, furniture, etc.
This invention relates to a method for producing a phenolic resin foam with excellent mechanical strength.
[従来の技術J
フェノール樹脂発泡体は、軽量で熱可塑性樹脂製発泡体
に比し、1t11!A性、耐熱性1機械的強度に優れ、
建材分野、家具等の材料として広く用いられる。[Conventional Technology J Phenolic resin foam is lighter and 1t11 lighter than thermoplastic resin foam! A property, heat resistance 1 excellent mechanical strength,
Widely used in the building material field and as a material for furniture, etc.
製造法としては、レゾール樹脂を原料とし、発泡剤とし
てトリクロルモノフルオロメタン(フロン−11)、1
−リクロルトリフルオロエタン(フロン−113)、ペ
ンタン等が主として用いられていた。The manufacturing method uses resol resin as a raw material, and uses trichloromonofluoromethane (Freon-11) and 1 as a blowing agent.
-Lichlorotrifluoroethane (Freon-113), pentane, etc. were mainly used.
しかし、フロン−11やフロン−113は発泡剤として
極めて優れた性質を有し1人体に対し無害で、引火性、
着火性もなく、工程的には安全な発泡剤ではあるが、こ
のフロン類が地球を取り巻くオゾン層を破壊し、地球の
環境破壊を促進することがわかり、使用量の減少、さら
には使用禁止の必要性が叫ばれつつある。However, Freon-11 and Freon-113 have extremely excellent properties as blowing agents, are harmless to the human body, and are flammable.
Although they are non-flammable blowing agents and are safe from a process standpoint, it has been discovered that these fluorocarbons destroy the ozone layer surrounding the earth and promote environmental destruction, leading to reductions in their usage and even banning their use. The need for this is becoming increasingly important.
また、ペンタンはフロンと異なり地球の環境破壊の問題
はないとしても、可燃性の炭化水素ガスであって、漏洩
すれば爆発や火災の危険の極めて大きい物質であり、ま
たその爆発範囲もペンタンが少量であってもその範囲に
入ること、空気より比重が重いため低所に貯り易く安全
上問題のあるガスであることはよく知られているところ
である。In addition, although pentane does not pose a problem of environmental destruction unlike fluorocarbons, it is a flammable hydrocarbon gas and poses an extremely high risk of explosion or fire if it leaks. It is well known that even a small amount of gas falls within this range, and that it is a gas that has a higher specific gravity than air, so it tends to accumulate in low places and poses a safety problem.
他の発泡剤としては加熱により窒素ガスを放出するアゾ
系化合物、ニトロン化合物等をノボラック型フェノール
樹脂に使用する方法があるが、これらの発泡剤をレゾー
ル型フェノール樹脂に配合した場合、樹脂の安定性が悪
(なり、また発泡剤が急激に反応分解してしまう等問題
が多く、また発泡直前に機械的に混合することも検討さ
れているが、発泡が急激で密度調整が難しくセル構造が
不安定な極めて外観の悪い発泡体しか得られない。Other blowing agents include azo compounds, nitrone compounds, etc. that release nitrogen gas when heated, and are used in novolac-type phenolic resins. However, when these blowing agents are blended with resol-type phenolic resins, the stability of the resin increases. There are many problems such as poor performance and rapid reaction and decomposition of the foaming agent.Additionally, mechanical mixing just before foaming has been considered, but foaming occurs rapidly and density adjustment is difficult, resulting in poor cell structure. Only unstable and extremely unsightly foams are obtained.
[発明が解決しようとする課題J
本発明はフェノール樹脂発泡体を製造する際に1発泡剤
として大気汚染・の原因となるフロン類、毒性の大きい
ハロゲン化炭化水素類を使用せず、また可燃性で爆発性
のあるペンタンのごとき炭化水素類を使用しないで耐熱
性、難燃性、断熱性、軽量性等の優れた特徴を持ったフ
ェノール樹脂発泡体を工業的に製造する方法の開発を目
的とする。[Problem to be Solved by the Invention J] The present invention does not use fluorocarbons that cause air pollution or highly toxic halogenated hydrocarbons as a blowing agent when manufacturing phenolic resin foam, and also does not use flammable halogenated hydrocarbons. Development of a method to industrially produce phenolic resin foam with excellent characteristics such as heat resistance, flame retardance, heat insulation, and lightness without using hydrocarbons such as pentane, which is highly explosive. purpose.
[課題を解決するための手段]
本発明は上記目的を達するために種々検討した結果、レ
ゾール型フェノール樹脂1発泡剤、整泡剤、酸硬化剤を
混合硬化してフェノール樹脂発泡体を製造するに当たり
、発泡剤としてスルホニルヒドラジン誘導体をレゾール
型フェノール樹脂100重量部に対し0.5〜45重量
部使用することを特徴とするフェノール樹脂発泡体の製
造法を開発した。[Means for Solving the Problems] As a result of various studies to achieve the above-mentioned object, the present invention has been developed to produce a phenolic resin foam by mixing and curing a resol type phenolic resin 1 blowing agent, a foam stabilizer, and an acid curing agent. For this purpose, we have developed a method for producing phenolic resin foam, which is characterized in that 0.5 to 45 parts by weight of a sulfonylhydrazine derivative is used as a blowing agent per 100 parts by weight of resol type phenolic resin.
またこの際に、フェノール樹脂が硬化する条件において
二酸化炭素を発生する化合物5例えば重炭酸ソーダ(重
ソウ)のごとき発泡剤を併用すること、更には発泡剤と
してスルホニルヒドラジン誘導体に二酸化炭素ガス又は
窒素ガスを併用(重ソウと3者の共用も可)することに
より、均一性のおる低密度の発泡体を得られる本発明を
完成した。In addition, at this time, a blowing agent such as a compound 5 that generates carbon dioxide under the conditions in which the phenol resin is cured, such as sodium bicarbonate, may be used, and carbon dioxide gas or nitrogen gas may be added to the sulfonylhydrazine derivative as a blowing agent. The present invention has been completed in which a homogeneous, low-density foam can be obtained by using them in combination (combined use of the three materials together with heavy sowing is also possible).
本発明で使用するレゾール型フエ、ノール樹脂の原料で
あるフェノール類としては1通常フェノール樹脂の製造
原料として用いられているフェノール、クレゾール、キ
シレノール等が挙げられるが、これらの中でも反応性、
硬化性の面からフェノール、メタクレゾールが特に好ま
しい、これらフェノール類は単独のみならず、これら同
士の混合、更に0−クレゾール、p−クレゾールまたビ
スフェノール等と併用しても良い。Examples of phenols that are raw materials for the resol-type phenol resins used in the present invention include phenol, cresol, xylenol, etc., which are usually used as raw materials for producing phenol resins.
From the viewpoint of curability, phenol and metacresol are particularly preferred. These phenols may be used not only alone, but also in combination with each other, or in combination with 0-cresol, p-cresol, bisphenol, or the like.
一方の原料としてのアルデヒド類としては、ホルムアル
デヒド、バラホルムアルデヒド、ポリオキシメチレン、
トリオキサン等が使用できる。この両者を塩基性触媒の
存在下に反応させ、脱水濃縮させてレゾール型フェノー
ル樹脂を得る。Aldehydes as raw materials include formaldehyde, paraformaldehyde, polyoxymethylene,
Trioxane etc. can be used. Both are reacted in the presence of a basic catalyst and dehydrated and concentrated to obtain a resol type phenol resin.
樹脂固型物としては60〜90%、粘度1.500〜δ
、000cps/25℃位が使用するのに便利であり、
もし濃縮度が高いときはアルコール、アセトン等で適宜
希釈して濃度、粘度を調整する。As a resin solid, 60-90%, viscosity 1.500-δ
,000cps/25℃ is convenient to use,
If it is highly concentrated, dilute it with alcohol, acetone, etc. to adjust the concentration and viscosity.
ここで発泡剤として使用するスルホニルヒドラジン誘導
体としては、構造式中に
−5−N−N<
■
を有する化合物であって、スルホニルヒドラジン誘導体
、スルホニルヒドラゾン誘導体等が含まれる。The sulfonylhydrazine derivative used as a blowing agent herein is a compound having -5-N-N<(2) in the structural formula, and includes sulfonylhydrazine derivatives, sulfonylhydrazone derivatives, and the like.
これらの化合物として例えば パラトルエンスルホニルヒドラジッド 0 CH。These compounds include e.g. paratoluenesulfonyl hydrazide 0 CH.
バラトルエンスルホニルアセトンヒドラゾン4.4°−
オキシビスベンゼンスルホニルヒドラジッド
があり、
分解したときのガスの主成分は窒素ガスである。Balatoluenesulfonylacetone hydrazone 4.4°-
There is oxybisbenzenesulfonyl hydrazide, and the main component of the gas when decomposed is nitrogen gas.
これらスルホニルヒ
ドラジン誘導体の使用量
は、フェノール樹脂100重量部に対して0.5〜45
重量部、好ましくは2〜20重量部使用する。The amount of these sulfonylhydrazine derivatives used is 0.5 to 45 parts by weight per 100 parts by weight of the phenol resin.
Parts by weight are used, preferably 2 to 20 parts by weight.
使用方法としては、限定はされないがあらかじめレゾー
ル型フェノール樹脂に整泡剤と共に混合してから硬化す
ることが発泡の均一性の面から好ましい態様である。Although the method of use is not limited, it is preferable from the viewpoint of uniformity of foaming to mix the resol type phenolic resin with a foam stabilizer in advance and then cure.
本発明に使用する整泡剤としては、フロン系発泡剤使用
の際に使用されていたものとほとんど同じものが用いら
れる。シリコーン系:エチレンオキサイド−プロピレン
オキサイド共重合体:ソルビタン、アルキルフェノール
またはヒマシ油等のポリオキシアルキレン付加物系等の
界面活性剤が使用できる。The foam stabilizer used in the present invention is almost the same as that used when using fluorocarbon foaming agents. Silicone-based: Ethylene oxide-propylene oxide copolymer: Surfactants such as sorbitan, alkylphenol, or polyoxyalkylene adducts such as castor oil can be used.
こわらは単独又は混合して使用されるが、使用量はフェ
ノール樹脂100重量部に対し、0.5〜IO重量部で
ある。The stiffeners may be used alone or in combination, and the amount used is 0.5 to IO parts by weight per 100 parts by weight of the phenolic resin.
酸硬化剤もフロン系発泡剤使用の際に使用されていたも
のと同じであって、例えばパラトルエンスルホン酸、フ
ェノールスルホン酸等の有機の強酸を使用する。添加量
はフェノール樹脂100重量部当たり5〜40重量部が
好ましい。The acid curing agent is the same as that used when using a fluorocarbon foaming agent, and for example, strong organic acids such as para-toluenesulfonic acid and phenolsulfonic acid are used. The amount added is preferably 5 to 40 parts by weight per 100 parts by weight of the phenolic resin.
発泡硬化させる方式も可能であるし、また整泡剤を含ん
だフェノール樹脂、酸硬化剤とスルホニルヒドラジン誘
導体をあらかじめ水有機溶剤に界面活性剤と共に分散し
て溶液にしたものをそれぞれ別々に連続的にフェノール
樹脂発泡機に供給し混合発泡硬化させることも可能であ
る。A foam curing method is also possible, or a phenol resin containing a foam stabilizer, an acid curing agent, and a sulfonylhydrazine derivative can be dispersed in advance in a water-organic solvent together with a surfactant to form a solution, and each can be prepared separately and continuously. It is also possible to supply the phenol resin to a foaming machine for mixing and foaming and curing.
また、発泡速度、発泡倍率をコントロールし易くするた
めスルホニルヒドラジン誘導体を共に他の発泡剤との併
用も可能で1例えば加熱や酸硬化剤のq在で分解して二
酸化炭素を発生する重ソウをレゾール型フェノール樹脂
100重量部に対し2〜20重1部を、スルホニルヒド
ラジン誘導体発泡剤と共に添加使用することで発泡速度
をコントロールし、良好な外観を持つ低密度発泡体を(
することか出来る。In addition, in order to make it easier to control the foaming rate and expansion ratio, sulfonylhydrazine derivatives can be used in combination with other foaming agents. By adding 1 part by weight of 2 to 20 parts by weight to 100 parts by weight of resol type phenolic resin together with a sulfonylhydrazine derivative blowing agent, the foaming speed can be controlled and a low density foam with a good appearance can be produced (
I can do something.
川に低密度、低コスト化のために引火性のないガスをス
ルホニルヒドラジン誘導体を併用する発泡剤として連続
的に発泡機を使用して供給することも可能で、この場合
入手し易さ1価格から二酸化炭素ガス、窒素ガスが有効
である0発泡剤として使用する二酸化炭素、窒素は液体
二酸化炭責、液化窒素の形で用いるのが便利で、フェノ
ール捌脂l容量部に対し、液化ガスの形で0.1容量部
〜30容量部位が適当である。It is also possible to continuously supply non-flammable gas to the river using a foaming machine as a foaming agent using a sulfonylhydrazine derivative in order to reduce density and cost.In this case, it is easy to obtain one price. It is convenient to use carbon dioxide and nitrogen gases as blowing agents in the form of liquid carbon dioxide or liquefied nitrogen. A suitable amount is 0.1 part to 30 parts by volume.
更に、発泡剤の分散を良好にするために溶媒を使用して
も良い、この場合、酸性下でCO8ガスを発生する液状
のアルキレンカーボネートが硬化を損なわず好適である
。Furthermore, a solvent may be used to improve the dispersion of the blowing agent. In this case, a liquid alkylene carbonate that generates CO8 gas under acidic conditions is preferred without impairing curing.
これらの硬化に際しては整泡剤及び/あるいはスルホニ
ルヒドラジン誘導体を含有したレゾール型フェノール樹
脂及び酸硬化剤を別々に連続的に)jノール樹脂発泡機
に供給すると共に急速に均一に混合しながらフェノール
樹脂発泡混合物を吐出させ、ついでモールド中で硬化さ
せることにより安全で大気汚染の全くないフェノール樹
脂発泡体を製造できる。During curing, a resol type phenolic resin containing a foam stabilizer and/or a sulfonylhydrazine derivative and an acid curing agent are separately and continuously supplied to a nord resin foaming machine, and the phenolic resin is rapidly and uniformly mixed. By discharging the foam mixture and then curing it in a mold, a safe and air-polluting phenolic resin foam can be produced.
この場合に使用するフェノール樹脂発泡体の混合機はフ
ロン系発泡剤を用いたときとほぼ同一の装置を採用でき
る。The mixer for the phenolic resin foam used in this case can be almost the same as that used when using a fluorocarbon foaming agent.
すなわち、整泡剤を含有する樹脂固型分及び粘度を調整
したレゾール型フェノール樹脂、発泡剤、酸硬化剤と、
フェノール樹脂発泡機に付属する定量ポンプで混合機(
ミキシングヘッド)に供給する0発泡剤は場合によって
はあらかじめフェノール樹脂に混合しておいてもよく、
ガス体の発泡剤はボンベ容器より定量的に直接ミキシン
グヘッドへ圧送供給も可能である。That is, a resol type phenolic resin containing a foam stabilizer with adjusted resin solid content and viscosity, a foaming agent, an acid curing agent,
Mixer (
In some cases, the blowing agent supplied to the mixing head) may be mixed with the phenolic resin in advance.
The blowing agent in the form of a gas can also be quantitatively supplied under pressure from a cylinder container directly to the mixing head.
ミキシングヘッドのスクリューは高速回転されており、
これら原料は瞬時に均一に混合され発泡機から押し出さ
れる。The mixing head screw is rotating at high speed,
These raw materials are instantly mixed uniformly and extruded from a foaming machine.
この発泡機からでた混合物は枠またはモールド中にて常
温〜100℃の温度で硬化される。The mixture from the foaming machine is cured in a frame or mold at temperatures ranging from room temperature to 100°C.
[作 用ル
ゾール型フェノール樹脂は硬化剤として強酸型の硬化剤
を使用するため、通常よく使用されている気体型(フロ
ン系)発泡剤が使用できる反面1分解型の発泡剤は使用
困難であった。[Function] Since Luzole type phenolic resin uses a strong acid type curing agent, commonly used gas type (fluorocarbon type) blowing agents can be used, but single decomposition type blowing agents are difficult to use. Ta.
しかるにスルホニルヒドラジン誘導体を発泡剤として使
用するときは、発泡条件が低温であるにも拘らず、比較
的スムーズに分解し、均一な発泡体を得ることができた
。However, when a sulfonylhydrazine derivative was used as a foaming agent, it decomposed relatively smoothly and a uniform foam could be obtained despite the low temperature foaming conditions.
更にこの場合、この条件下において重ソウのごとく二酸
化炭素を放出する化合物を併用するときは発泡速度1発
泡倍率のコントロールも容易となることが分かった。Furthermore, in this case, it has been found that under these conditions, when a compound that releases carbon dioxide, such as sodium chloride, is used in combination, it becomes easy to control the foaming rate and foaming ratio.
さらに二酸化炭素、窒素を発泡剤として併用するときも
同じような効果をもたらすことが分かった。Furthermore, it was found that similar effects can be produced when carbon dioxide and nitrogen are used in combination as blowing agents.
次に実施例を示し、本発明を更に具体的に説明する。EXAMPLES Next, the present invention will be explained in more detail with reference to Examples.
[実施例J
(実施例1)
四ツロフラスコにフェノール2Kg、37%ホルムアル
デヒド2.93Kg (ホルムアルデヒド/フェノール
二モル比1.7モル)及び触媒として20%力性ソーダ
60gを仕込み、80’Cで3時間反応した後、15%
硫酸でpHを7.0に中和し、減圧脱水により樹脂中の
水分を5%以下にした。[Example J (Example 1) 2 kg of phenol, 2.93 kg of 37% formaldehyde (formaldehyde/phenol dimolar ratio 1.7 mol) and 60 g of 20% sodium chloride as a catalyst were placed in a four-sided flask, and heated at 80'C for 30 minutes. After reacting for an hour, 15%
The pH was neutralized to 7.0 with sulfuric acid, and the water content in the resin was reduced to 5% or less by dehydration under reduced pressure.
得られたレゾール型フェノール樹脂は樹脂固形分80%
、粘度2500 c p s / 25℃、比重1.2
5/25℃、ff1lt平均分子J!t430−cアラ
た。The obtained resol type phenolic resin has a resin solid content of 80%.
, viscosity 2500 cps/25℃, specific gravity 1.2
5/25℃, ff1lt average molecule J! t430-c Arata.
このレゾール型フェノール樹脂100重量部に対して整
泡剤としてトウィーンNo、40(ポリオキシエチレン
ソルビタンモノパルミテート)2重量部を混合し、レゾ
ール型発泡用フェノール樹脂とした。2 parts by weight of Tween No. 40 (polyoxyethylene sorbitan monopalmitate) as a foam stabilizer was mixed with 100 parts by weight of this resol type phenolic resin to obtain a resol type phenol resin for foaming.
得られた発泡用フェノール樹脂100重量部に発泡剤−
K(セルマイク−に;主成分パラトルエンスルホニルア
セトヒドラゾン〈ニー化成))を5重量部混合した後、
65%フェノールスルホンal(PSA)15重量部を
フェノール樹脂発泡機により急速に均一に混合し、幅5
0cm、長さ25cm、高さ4cmの鉄枠中に一定量流
し込み、これを40℃オーブン中で5分間放置し、発泡
硬化を完了させてフェノール樹脂発泡体を得た。A blowing agent was added to 100 parts by weight of the obtained foaming phenolic resin.
After mixing 5 parts by weight of K (into Cellmic; main component para-toluenesulfonylacetohydrazone (Nie Kasei)),
15 parts by weight of 65% phenol sulfone al (PSA) was rapidly and uniformly mixed using a phenol resin foaming machine, and
A certain amount of the mixture was poured into an iron frame measuring 0 cm, length 25 cm, and height 4 cm, and this was left in an oven at 40° C. for 5 minutes to complete foaming and curing to obtain a phenolic resin foam.
得られたフェノール樹脂発泡体の物性は密度45Kg/
m”、吸水量4.0g7100cm”熱伝導率0.02
8Kcal/m−hr・”cであり、外観上も全体的に
均一であった。The physical properties of the obtained phenolic resin foam have a density of 45 kg/
m", water absorption 4.0g7100cm" thermal conductivity 0.02
It was 8Kcal/m-hr·''c, and the appearance was uniform throughout.
(実施例2〜4.比較例1)
実施例1と同条件で製造された整泡剤添加済レゾール型
発泡用フェノール樹脂100重量部に発泡剤−にの添加
量を変えた結果及び発泡剤−F■(セルマイク−■、パ
ラトルエンスルボニルヒドラジッド〈ニー化成))、発
泡剤−3(セルマイク−5;4.4°−オキシビスベン
ゼンスルホニルヒドラジッド〈ニー化成))を使用した
結果を第1表に示す。(Examples 2 to 4. Comparative Example 1) Results of changing the amount of foaming agent added to 100 parts by weight of a resol-type foaming phenolic resin with foam stabilizer added manufactured under the same conditions as Example 1, and the results of changing the amount of foaming agent added - F Shown in Table 1.
(以下余白)
第
表
(実施例5)
実施例1と同条件で製造されたレゾール型発泡用フェノ
ール樹脂100重量部に発泡剤−に4重量部と重ソウ4
重量部を混合した後、65%フェノールスルホン111
18重量部をフェノール樹脂発泡機により急速に均一混
合し1幅50cm、長さ25cm、高さ4cmの鉄枠中
に一定量流し込み、これを40℃オーブン中で5分間放
置し1発泡硬化を完了させてフェノール樹脂発泡体を得
た。得られたフェノール樹脂発泡体の物性は密度35K
g/m”、吸水量4.0g/100cm”熱伝導率0.
027Kcal/m−hr・”cであり外観上も全体に
均一であった。(Leaving space below) Table (Example 5) 100 parts by weight of a resol-type foaming phenolic resin produced under the same conditions as Example 1, 4 parts by weight of a blowing agent, and 4 parts by weight of heavy sodium chloride.
After mixing parts by weight, 65% phenolsulfone 111
18 parts by weight were quickly and uniformly mixed using a phenolic resin foaming machine, and a certain amount was poured into an iron frame with a width of 50 cm, a length of 25 cm, and a height of 4 cm, and this was left in an oven at 40°C for 5 minutes to complete foam curing. A phenolic resin foam was obtained. The physical properties of the obtained phenolic resin foam are that the density is 35K.
g/m", water absorption 4.0 g/100 cm", thermal conductivity 0.
027 Kcal/m-hr·"c, and the appearance was uniform throughout.
(実施例6,7、比較例2)
実施例5と同法で発泡剤−K、重ソウの添加量を変えた
結果を第2表に示す。(Examples 6 and 7, Comparative Example 2) Table 2 shows the results of the same method as in Example 5, but with different amounts of blowing agent-K and heavy sodium chloride.
第
表
(以下余白)
(実施例8)
実施例1と同一の組成の整泡剤添加済レゾール型発泡用
フェノール樹脂1.6β/ m i nに対し65%フ
ェノールスルホンM(比重1.35)0.26ff/m
in及び発泡剤−A[発泡剤−に/プロピレンカーボネ
ート/トウィーンN。Table (blank space below) (Example 8) 65% phenol sulfone M (specific gravity 1.35) for resol type foaming phenol resin 1.6β/min with foam stabilizer added having the same composition as Example 1 0.26ff/m
in and blowing agent-A [blowing agent-in/propylene carbonate/Tween N.
40=2/2/1の混合液1を0.16β/m i n
をフェノール樹脂発泡機の定量ポンプより混合機(ミキ
シングヘッド)に供給し、フェノル樹脂、フェノールス
ルホン酸1発泡剤−八を瞬時に均一混合し、混合機底口
より吐き出し1幅50cm、長さ25cm、高さ4cm
の鉄枠中に一定量流し込み、これを40℃オーブン中で
5分間放置し、発泡硬化を完−rしてフェノール樹脂発
泡体を得た。40=2/2/1 mixture 1 at 0.16β/min
is supplied to the mixer (mixing head) from the metering pump of the phenol resin foaming machine, and the phenol resin, phenol sulfonic acid 1 blowing agent-8 are instantly and uniformly mixed, and the mixture is discharged from the bottom of the mixer into a 50 cm wide and 25 cm long foam. , height 4cm
A certain amount of the mixture was poured into an iron frame, and the mixture was left in an oven at 40° C. for 5 minutes to completely cure the foam, thereby obtaining a phenolic resin foam.
得られたフェノール樹脂発泡体の物性は密度35 K
g / m ” 、吸水量4. 1 g/ l 00c
+i”熱伝導率0.028Kcal/m−hr・”cで
あり、外観上も全体に均一であった。The physical properties of the obtained phenolic resin foam are that the density is 35K.
g/m”, water absorption 4.1 g/l 00c
+i'' Thermal conductivity was 0.028 Kcal/m-hr·''c, and the appearance was uniform throughout.
(実施例9)
実施例8と同法でミキシングヘッドにフェノール樹脂1
.6g/min、65%フェノールスルホン酸0.26
g/min、発泡剤−Ao、16ff/minを供給し
、液体二酸化炭素1.6β/minを別ラインより混合
機に注入し、各成分を瞬時に均一混合し、実施例8と同
じ方法で発泡硬化させてフェノール樹脂発泡体を得た。(Example 9) Phenol resin 1 was added to the mixing head using the same method as in Example 8.
.. 6g/min, 65% phenolsulfonic acid 0.26
g/min, blowing agent-Ao, 16ff/min, liquid carbon dioxide 1.6β/min was injected into the mixer from a separate line, each component was instantly and uniformly mixed, and the same method as Example 8 was carried out. A phenolic resin foam was obtained by foaming and curing.
得られたフェノール樹脂発泡体の物性は密度20Kg/
m”、吸水1t4 、 Og/ 100cm”熱伝導率
0.027Kcal/m−hr−’Cであり、外観上も
全体的に均一であった。The physical properties of the obtained phenolic resin foam have a density of 20 kg/
m", water absorption of 1 t4, Og/100 cm", thermal conductivity of 0.027 Kcal/m-hr-'C, and the overall appearance was uniform.
(実施例10)
実&i例9と同法で液体二酸化炭素の量を20β/mi
nに変えた結果を第3表に示す。(Example 10) The amount of liquid carbon dioxide was adjusted to 20β/mi using the same method as Example 9.
Table 3 shows the results after changing n.
(実施例11)
実施例1で得た同じ組成の整泡剤添加済みのレゾール型
発泡用樹脂100重量部に更に発泡剤−に4重量部をあ
らかじめ混合した発泡剤添加済レゾール型発泡用フェノ
ール樹脂1.6ε/min、65%フェノールスルホン
酸0.262/minの割合で混合機に供給すると共に
二酸化炭素3.OI2/minを実施例9と同法で均一
混合し発泡硬化させフェノール樹脂発泡体を得た。(Example 11) A phenol for resol type foaming with a foaming agent added, which was prepared by pre-mixing 100 parts by weight of the resin for resol type foaming with the same composition as in Example 1 with the addition of a foam stabilizer and 4 parts by weight of a blowing agent. The resin is fed to the mixer at a rate of 1.6ε/min and the 65% phenolsulfonic acid is fed at a rate of 0.262/min, while carbon dioxide is fed at a rate of 3. OI2/min was uniformly mixed in the same manner as in Example 9, and the mixture was foamed and cured to obtain a phenol resin foam.
得られた発泡体の物性は密度18Kg/m”吸水量4.
0g/100cm”、熱伝導率0.027Kcal/m
−hr・”cで外観も均一良好であった。The physical properties of the obtained foam were as follows: density: 18 Kg/m" water absorption: 4.
0g/100cm", thermal conductivity 0.027Kcal/m
The appearance was uniform and good at -hr・”c.
(実施例!2.13.比較例3〜5、参考例1)実施例
11と同一方法であって、二酸化炭素ガス(液体二酸化
炭素換算)の供給量、窒素ガスの供給量を変えた場合の
結果を第3表に示す。(Example! 2.13. Comparative Examples 3 to 5, Reference Example 1) Same method as Example 11, but with different supply amount of carbon dioxide gas (liquid carbon dioxide equivalent) and nitrogen gas supply amount The results are shown in Table 3.
なお、参考のためフロン−113を使用し、本発明の実
施例とほぼ同一の製品を得る条件を示す。For reference, Freon-113 is used and conditions for obtaining a product almost the same as in the examples of the present invention are shown.
(以下余白)
【発明の効果]
従来1発泡剤として使用されていたトリクロルモノフル
オロメタン(フロン−11)、l−リクロルトリフルオ
ロエタン(フロン−113)はオゾン層を破壊し、地球
の環境汚染をするとされて使用量の制限、使用禁止の必
要が叫ばれており、フロンを使用しない製造法の開発が
要望されていた。(Left below) [Effects of the invention] Trichloromonofluoromethane (Freon-11) and l-lychlortrifluoroethane (Freon-113), which were conventionally used as blowing agents, destroy the ozone layer and harm the global environment. There have been calls for the use of chlorofluorocarbons to be restricted or banned as they are thought to pollute, and there has been a demand for the development of a manufacturing method that does not use fluorocarbons.
これに対し本発明は、発泡剤の出発原料としてスルホニ
ルヒドラジン誘導体又はそれと硬化条件下において二酸
化炭素を発生する化合物、液化二酸化炭素、液体窒素を
併用することにより、樹脂の安定性、セル構造の均一性
、良好な外観1発泡速度、発泡倍率のコントロール等操
業の容易性に優れた発泡剤を見出し、大気汚染をなくシ
、また爆発の危険なく、安全にフェノール樹脂発泡体の
製造を可能とする技術を開発した。In contrast, the present invention uses a sulfonylhydrazine derivative or a compound that generates carbon dioxide under curing conditions, liquefied carbon dioxide, or liquid nitrogen in combination as a starting material for the blowing agent, thereby stabilizing the resin and achieving a uniform cell structure. We have discovered a foaming agent that has excellent operability such as control of foaming speed and expansion ratio, and enables the safe production of phenolic resin foam without air pollution or the risk of explosion. developed the technology.
特許出願人 昭和高分子株式会社Patent applicant: Showa Kobunshi Co., Ltd.
Claims (5)
硬化剤を混合硬化してフェノール樹脂発泡体を製造する
に当たり、発泡剤としてスルホニルヒドラジン誘導体を
レゾール型フェノール樹脂100重量部に対し0.5〜
45重量部使用することを特徴とするフェノール樹脂発
泡体の製造法。(1) When producing a phenolic resin foam by mixing and curing a resol-type phenolic resin, a blowing agent, a foam stabilizer, and an acid curing agent, 0.00% of a sulfonylhydrazine derivative is added as a blowing agent to 100 parts by weight of the resol-type phenolic resin. 5~
A method for producing a phenolic resin foam, characterized in that 45 parts by weight is used.
するフェノール樹脂発泡体の製造法において、二酸化炭
素を発生する発泡剤を併用する請求項(1)のフェノー
ル樹脂発泡体の製造法。(2) The method for producing a phenolic resin foam according to claim (1), wherein in the method for producing a phenolic resin foam using a sulfonylhydrazine derivative as a blowing agent, a blowing agent that generates carbon dioxide is used in combination.
する請求項(1)または(2)記載のフェノール樹脂発
泡体の製造法において、炭酸ガスを発泡剤として併用す
るフェノール樹脂発泡体の製造法。(3) The method for producing a phenolic resin foam according to claim (1) or (2), wherein a sulfonylhydrazine derivative is used as a blowing agent, in which carbon dioxide gas is used in combination as a blowing agent.
する請求項(1)または(2)記載のフェノール樹脂発
泡体の製造法において、窒素を発泡剤として併用するフ
ェノール樹脂発泡体の製造法。(4) The method for producing a phenolic resin foam according to claim (1) or (2), wherein a sulfonylhydrazine derivative is used as a blowing agent, in which nitrogen is also used as a blowing agent.
する請求項(1)ないし(4)記載のフェノール樹脂発
泡体の製造法において、分散溶媒としてアルキレンカー
ボネートを用いるフェノール樹脂発泡体の製造法。(5) A method for producing a phenolic resin foam according to any of claims (1) to (4), wherein a sulfonylhydrazine derivative is used as a blowing agent, and an alkylene carbonate is used as a dispersion solvent.