JPS5828016A - 複層軸受 - Google Patents
複層軸受Info
- Publication number
- JPS5828016A JPS5828016A JP56126125A JP12612581A JPS5828016A JP S5828016 A JPS5828016 A JP S5828016A JP 56126125 A JP56126125 A JP 56126125A JP 12612581 A JP12612581 A JP 12612581A JP S5828016 A JPS5828016 A JP S5828016A
- Authority
- JP
- Japan
- Prior art keywords
- porous layer
- metal
- back metal
- composite
- ptfe
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
め要約のデータは記録されません。
Description
【発明の詳細な説明】
本発明は、複層軸受の改良に関するものである。
従来の複層軸受としては、例えば特開昭54−4544
0号公報が存在する。まずこの従来の複層軸受について
説明すると、金属裏金に裏打ちされた多孔質層とその表
面に、重量で4ぶつ化エチレン−6ぶつ化プロピレン共
重合樹脂(以下、FEPという)5〜40Xと、残部が
実質的にPTFE(60〜95%)からなる組成物を含
浸および被覆してなる複層軸受である。
0号公報が存在する。まずこの従来の複層軸受について
説明すると、金属裏金に裏打ちされた多孔質層とその表
面に、重量で4ぶつ化エチレン−6ぶつ化プロピレン共
重合樹脂(以下、FEPという)5〜40Xと、残部が
実質的にPTFE(60〜95%)からなる組成物を含
浸および被覆してなる複層軸受である。
しかしながら、この従来の複層軸受は、すべり軸受特性
にとって極めて重要な耐キャビテーション性(潤滑油中
において、ガスの析出または蒸気が生成し、このガスま
たは蒸気がたとえ軸受摺動面や軸受端面を高速度で激し
く衝撃しても、摩耗、剥離、亀裂などの損傷に耐え得る
性質をいう。)、耐摩耗性および低摩擦性は必ずしも満
足すべきものではなかった。
にとって極めて重要な耐キャビテーション性(潤滑油中
において、ガスの析出または蒸気が生成し、このガスま
たは蒸気がたとえ軸受摺動面や軸受端面を高速度で激し
く衝撃しても、摩耗、剥離、亀裂などの損傷に耐え得る
性質をいう。)、耐摩耗性および低摩擦性は必ずしも満
足すべきものではなかった。
本発明の目的は、この従来の複層軸受よりも耐キャビテ
ーション性、耐摩耗性および低摩擦性の一層すぐれた複
層軸受を提供することにある。
ーション性、耐摩耗性および低摩擦性の一層すぐれた複
層軸受を提供することにある。
すなわち、本発明の要旨とするところは、金属裏金に裏
打ちされた多孔質層とその表面に、ニルエーテル共重合
樹脂(以下、PFAとい% ’)]j゛、0.1〜50
%と、残部が実質的にPTFE(50〜999%)から
なる組成物を含浸および被覆してなる複層軸受である。
打ちされた多孔質層とその表面に、ニルエーテル共重合
樹脂(以下、PFAとい% ’)]j゛、0.1〜50
%と、残部が実質的にPTFE(50〜999%)から
なる組成物を含浸および被覆してなる複層軸受である。
本発明の特徴とするところは、従来の複層軸受の含浸被
覆用組成物におけるFEPO代わりにPFAを使用した
点にある。すなわち、本発明者はPFAがFEPよりも
、主成分のPTFEや金属裏金との接着性(粘着性)の
良好なことを試行錯誤により見い出したのである。
覆用組成物におけるFEPO代わりにPFAを使用した
点にある。すなわち、本発明者はPFAがFEPよりも
、主成分のPTFEや金属裏金との接着性(粘着性)の
良好なことを試行錯誤により見い出したのである。
次に、本発明の複層軸受における含浸被覆用組成物を、
前記特許請求の範囲に記載のごとく限定する理由(上限
、下限の決定理由)と、その作用効果について説明する
と、PFAo、1容量%以下の場合は、耐摩耗性および
本発明の目的である耐キャビテーション性が著しく低下
する。まだ50容量%を越えるとPFAが主成分となり
、耐キャビテーション性、耐摩耗性が向上するけれども
、摩擦係数と摩擦温度が上昇して、軸受性能を低下させ
るので、50容量%を限度とした。
前記特許請求の範囲に記載のごとく限定する理由(上限
、下限の決定理由)と、その作用効果について説明する
と、PFAo、1容量%以下の場合は、耐摩耗性および
本発明の目的である耐キャビテーション性が著しく低下
する。まだ50容量%を越えるとPFAが主成分となり
、耐キャビテーション性、耐摩耗性が向上するけれども
、摩擦係数と摩擦温度が上昇して、軸受性能を低下させ
るので、50容量%を限度とした。
以下、実施例について説明する。
実施例
銅メッキを施した鋼裏金上に青銅粉末を多孔質に焼結し
、しかる後、表1に示しだ含浸被覆用組成物を塗布後、
ロール間に通して前記多孔質青銅層の孔隙とその表面に
前記組成物を含浸および被覆させ、次いで627〜40
0’Cの温度で焼成し、さらにロールを通過させて厚み
を均一にして従来品(試料A1〜4)および本発明品(
試料屋5〜8)を得た。
、しかる後、表1に示しだ含浸被覆用組成物を塗布後、
ロール間に通して前記多孔質青銅層の孔隙とその表面に
前記組成物を含浸および被覆させ、次いで627〜40
0’Cの温度で焼成し、さらにロールを通過させて厚み
を均一にして従来品(試料A1〜4)および本発明品(
試料屋5〜8)を得た。
このものの試験条件とその試験結果をそれぞれ表2、表
6に示し、摩擦摩耗試験条件とその試験結果をそれぞれ
表4、表5に示した。
6に示し、摩擦摩耗試験条件とその試験結果をそれぞれ
表4、表5に示した。
なお、本発明に使用される裏金は鋼以外の金属でもよく
、丑だ裏金にはメッキなしか、まだは銅メツキ以外の他
の金属、合金メッキでもよく、また裏金に形成される多
孔質層は青銅など銅系合金以外の他の金属、合金を用い
てもよい。
、丑だ裏金にはメッキなしか、まだは銅メツキ以外の他
の金属、合金メッキでもよく、また裏金に形成される多
孔質層は青銅など銅系合金以外の他の金属、合金を用い
てもよい。
まだ、本発明の用途は、液体中で作動する特にキャビテ
ーションが発生する条件下で作動する個所に最適である
。例えばショックアブソーバ用である。
ーションが発生する条件下で作動する個所に最適である
。例えばショックアブソーバ用である。
次に、前記の実施例における作用効果について詳しく説
明する。
明する。
表6と表5かられかるように、従来品(試料A1−扁4
)と、本発明品(試料屋5〜屋8)と比較(ただし、同
一含有量同士と比較する。
)と、本発明品(試料屋5〜屋8)と比較(ただし、同
一含有量同士と比較する。
すなわち、試料A2と試料Jf66と比較、試料屋6と
試料A7と比較、試料A4と試料A8と比較)すると、
キャビテーションによる軸受摺動面の体積減量および摩
耗量、摩擦係数は、本発明品のほうが約1/2ないしそ
れ以下に改善されており、さらに従来品の試料扁1と本
発明品屋5〜A8と比較すると、本発明品のほうが耐キ
ャビテーション性、耐摩耗性および低摩擦性がすこぶる
改善されており、本発明は所期の目的を達成することが
できる。
試料A7と比較、試料A4と試料A8と比較)すると、
キャビテーションによる軸受摺動面の体積減量および摩
耗量、摩擦係数は、本発明品のほうが約1/2ないしそ
れ以下に改善されており、さらに従来品の試料扁1と本
発明品屋5〜A8と比較すると、本発明品のほうが耐キ
ャビテーション性、耐摩耗性および低摩擦性がすこぶる
改善されており、本発明は所期の目的を達成することが
できる。
表 1
表 2
表 6
表 4
表 5
特許出願人 大同メタル工業株式今社手続補正書(自
発) 1、事件の表示 昭和56年特許願第126125号 2、発明の名称 複層軸受 6、補正をする者 事件との関係 特許出願人 名 称 笑開メタル貴株式会社 4、補正の対象 (1)明細書「特許請求の範囲」
の欄(2)明細書「発明の詳細な説明」の欄(1)
明細書「特許請求の範囲」の記載を別紙のとおり補正す
る。
発) 1、事件の表示 昭和56年特許願第126125号 2、発明の名称 複層軸受 6、補正をする者 事件との関係 特許出願人 名 称 笑開メタル貴株式会社 4、補正の対象 (1)明細書「特許請求の範囲」
の欄(2)明細書「発明の詳細な説明」の欄(1)
明細書「特許請求の範囲」の記載を別紙のとおり補正す
る。
(2) 明細書「発明の詳細な説明」の欄を次のとお
り補正する。
り補正する。
1、 第2頁第15行中「′4ぶつ化エチレン−パー7
0ロアキルビ」を「4ふつ化エチレン−パーフロロアル
キルビ」と訂正する。
0ロアキルビ」を「4ふつ化エチレン−パーフロロアル
キルビ」と訂正する。
2、特許請求の範囲
金属裏金に裏打ちされた多孔質層とその表面K、容量%
で4ふつ化エチレンーパー70ロアルキルビニルエーテ
tv共重合樹脂0.1〜50%と、残部が実質的にPT
FEからなる組成物を含浸および被覆してなる複層軸受
。
で4ふつ化エチレンーパー70ロアルキルビニルエーテ
tv共重合樹脂0.1〜50%と、残部が実質的にPT
FEからなる組成物を含浸および被覆してなる複層軸受
。
92−
Claims (1)
- 金属裏金に裏打ちされた多孔質層とその表面に、容量%
で4ぶつ化エチレンーパー70ロアキルビニルエーテル
共重合l脂0.1〜50%と、残部が実質的にPTFE
からなる組成物を含浸および被覆してなる複層軸受。