JPS6024502A - 位相差板 - Google Patents

位相差板

Info

Publication number
JPS6024502A
JPS6024502A JP13320683A JP13320683A JPS6024502A JP S6024502 A JPS6024502 A JP S6024502A JP 13320683 A JP13320683 A JP 13320683A JP 13320683 A JP13320683 A JP 13320683A JP S6024502 A JPS6024502 A JP S6024502A
Authority
JP
Japan
Prior art keywords
retardation plate
phase difference
thickness
difference plate
polyolefin resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP13320683A
Other languages
English (en)
Inventor
Junichi Fujio
藤生 順一
Makoto Hosonuma
細沼 信
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsui Toatsu Chemicals Inc
Original Assignee
Mitsui Toatsu Chemicals Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsui Toatsu Chemicals Inc filed Critical Mitsui Toatsu Chemicals Inc
Priority to JP13320683A priority Critical patent/JPS6024502A/ja
Publication of JPS6024502A publication Critical patent/JPS6024502A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 本発明は耐湿恰、耐熱にすぐれた新規な位相差板に関す
るものである。
、位相差板とは、複屈折性を有する板状体であシ、光線
が透過した場合に互に直交する二方向の屈折率の違いに
より互に直交する光線の位相がずれるものである。特に
、入射光線の波長(λ)に対して1/4λ分だけ位相差
を生ずるようにした位相差板を1/4λ板と呼んでいる
。
この174λ板の軸に対し、直線偏光板の軸を45゜傾
けて貼シ合せた複合板は通過する自然光を円偏光に変換
する機能を有しておシ、円偏光板と呼ばれ、光線を反射
する物体の前面に配置すると反射光線をほぼ完全に消滅
する効果があるので、各種表示装置の光線反射防止、防
眩用材料として用いられている。
この位相差板としては、複屈折性を有する無機結晶性物
質、例えば水晶、方解石などを薄い板状にしたものが用
いられている。この無機物質でできた位相差板は高度に
均質であシ、耐湿性、耐熱性が養いので良好に用いうる
のであるが、可撓性がないこと、また、大きなものを作
るには格子欠陥のほとんどない大きな結晶がいることな
どから高価となると七等の欠点がある。
一方、プラスチック材料では延伸すると簡単に複屈折を
示すものがあシ、良好な材料となシうると推定されるの
であるが、光学的に均一な性質を有するほどに延伸する
と複屈折性が過大になる欠点がアシ、実用に供されてい
るものとして、天然物のセルロースの誘導体であるセル
ロースアセテート系のものがあるのみである。
ところで、このセルロースアセテートハ吸湿性が強く、
高湿度下で用いると吸湿により複屈折性が大巾に変化す
るという欠点を有すると共に、高温化でも変質しやすい
という欠点がある。
本発明の目的は安価で耐湿性、耐熱性に優れたプラスチ
ック製の位相差板を提供することにある。
本発明者らはかかる実情下に位相差板の材料につき鋭意
検討した結果、意外にもポリオレフィン樹脂を用いたな
らば良好な位相差板を作成しうろことを見出し、更に研
究して遂に本発明を完成するに到った。
−即ち、本発明はポリオレフィン樹脂からなる位相差板
である。
本発明に用いるポリオレフィン樹脂とは、エチレン、プ
ロピレン、1−ブテン等のα−オレフィンを重合させた
ものであシ、単独重合体はもちろんこれらα−オレフィ
ンの共重合体でも使用できる。光学的特性の点で共重合
体の方が好ましい。
共重合ポリオレフィン樹脂としてはプロピレンとエチレ
ンの共重合体が好ましいものであシ、中でもエチレンを
2〜15モル%のものが更に好ましい。この範囲のプロ
ピレン−エチレン共重合体では特に透明性、結晶化の程
度、耐熱性が良好であシ、加工性も良好である。
ポリオレフィン樹脂を位相差板とするには、ポリオレフ
ィン樹脂に必要に応じ安定剤、紫外線吸収剤、核剤、滑
剤、流滴剤等を加え、一般のTダイ押出し、インフレー
ション等の方法で厚さ25〜500μmのフィルムとす
ることにより達成さする。
ポリオレフィン樹脂によっては結晶化がはげしくて大き
な球晶を発生しやすく、位相差板とじて不適なものとな
りやすいので、いわゆる核剤を加えておくことが透明性
等の改善の上で好ましい。
ところで、ポリオレフィン樹脂を単にフィルムにしただ
けでは位相差板として適したものは得らrしず、例えば
Tダイ押出しで位相差板を作成するには、Tダイの吐出
口から押出された樹脂が冷却されながら幾分延伸される
ように引き取られることが望ましい。
Tダイの吐出口から押出された樹脂厚みと引取冷却され
たフィルム厚みの比(ドロー比)は得ようとする位相差
板の厚み、複屈折の程度により異なるが通常4〜50の
範囲が適当である。
このようにして得られたフィルムは更に熱固定して歪を
除去して位相差板として用いる。
本発明の位相差板はポリオレフィン樹脂でできているの
で耐湿性に優れているのはもちろん、耐熱性もちフ、か
つ、光学的特性も優れている。
更に、本発明の位相差板は目的とする位相差を得るため
には厚み、ドロー比を変えることによシ容易に製造する
ことが可能である点も優れている。
本発明の位相差板で特に位相差を自然光の平均波長(λ
= 540 nm)の1/4、すなわち約135nmK
g節したいわゆる1/4λ板は、偏光板と組合せて円偏
光板として各種表示装置の防眩用に利用価値が太きいも
のである。
以下、実施例によシ本発明を説明する。
実施例1゜ エチレンを6モル2共重合したポリプロピレン樹脂″三
井ノーブレンMJS−G” (商標、MI=1.5F/
10分)に核剤としてジ(p−エチルベンジリデン)ン
ルビトールを0.1重量%配合したものを、40φ押出
機で溶融製膜を行った。得られたフィルムの光学的特性
を測定し、表−IK示す結果をえた。押出条件は以下の
通りであった。
な・お、これらの中で位相差が135 nm付近にある
ものはIAλ板として、防眩効果にすぐれたものであっ
た。
表−1 *I Tダイリップ出口の線速度を示す。
*2 ドロー比−Tダイリッグ巾(0,8ny’in)
/フィルム厚み(Mm)*3 常法に従い偏光顕微鏡を
用いてセメルモン方式で測定した。
*4 JIS K−6718による。
また、高温・高湿下においた(80℃、95%RH,5
00時間)場合の変化を調べたところ、実施例1で得ら
れた位相差板ではほとんど変化がなく良好であった。一
方、同時に市販のセルロース系のものでは、収縮、白濁
が見らt1上記条件においたのちに測定した位相差は大
きく変化していた。
特許出願人 三井東圧化学株式会社

Claims (1)

  1. 【特許請求の範囲】 1、 ポリオレフィン樹脂からなることを特徴とする位
    相差板。 2、ポリオレフィン樹脂がα−オレフィンを共重合した
    ものである特許請求の範囲第1項記載の位相差板。 3、共重合ポリオレフィン樹脂がプロピレンとエチレン
    の共重合樹脂である特許請求の範囲第2項記載の位相差
    板。 4、プロピレンとエチレンの共重合樹脂がエチレン含有
    量が2〜15モル%のものである特許請求の範囲第3項
    記載の位相差板。 5、ポリオレフィン樹脂の厚みが25〜500μmであ
    る特許請求の範囲第1項記載の位相差板。
JP13320683A 1983-07-21 1983-07-21 位相差板 Pending JPS6024502A (ja)