JPS64281A - オーバレイ・コーティング - Google Patents
オーバレイ・コーティングInfo
- Publication number
- JPS64281A JPS64281A JP63070831A JP7083188A JPS64281A JP S64281 A JPS64281 A JP S64281A JP 63070831 A JP63070831 A JP 63070831A JP 7083188 A JP7083188 A JP 7083188A JP S64281 A JPS64281 A JP S64281A
- Authority
- JP
- Japan
- Prior art keywords
- protective layer
- coating
- particles
- particle size
- weight
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
め要約のデータは記録されません。
Description
【発明の詳細な説明】
産業上の利用分野
本発明は、支持体上に熱障壁を結合するオーバレイ・コ
ーティングの提供に関する。上記のオーバレイ・コーテ
ィングは、特に腐食や浸食が発生しそうな高温環境にさ
らされる構成部分に用いられるが、上記コーティングの
主要な、但し必ずしも唯一ではない応用は、ガスタービ
ン・エンジンの部品、特にガスタービンの燃焼筒製品、
静翼および動翼、ならびに案内羽根に対するものである
。
ーティングの提供に関する。上記のオーバレイ・コーテ
ィングは、特に腐食や浸食が発生しそうな高温環境にさ
らされる構成部分に用いられるが、上記コーティングの
主要な、但し必ずしも唯一ではない応用は、ガスタービ
ン・エンジンの部品、特にガスタービンの燃焼筒製品、
静翼および動翼、ならびに案内羽根に対するものである
。
従来の技術
適宜に作られた支持体表面に、プラズマ析出プロセスを
用いて、MCrAj!Y (ここにMはニッケルもしく
はコバルト、またはニッケルおよびコバルトなどの適当
な金属)から成る保護層を最初に噴霧コーティングし、
次いで保護か内のそれよりも可成り粗大な粒子を析出物
内に生成するフレーム析出ブOセスにより金属から成る
固着層を噴霧コーティングし、次いでプラズマ析出プロ
゛セスにより耐火物から成る熱障壁を噴霧コーティング
することによってオーバレイ・コーティングを生成する
ことが提案されている。
用いて、MCrAj!Y (ここにMはニッケルもしく
はコバルト、またはニッケルおよびコバルトなどの適当
な金属)から成る保護層を最初に噴霧コーティングし、
次いで保護か内のそれよりも可成り粗大な粒子を析出物
内に生成するフレーム析出ブOセスにより金属から成る
固着層を噴霧コーティングし、次いでプラズマ析出プロ
゛セスにより耐火物から成る熱障壁を噴霧コーティング
することによってオーバレイ・コーティングを生成する
ことが提案されている。
発明が解決しようとする問題点
この手順は概して申し分のないものであるが、これには
若干の理想的でない面がある。例えば、複雑で内的する
表面に対するフレーム噴霧は困難且つ高価となる可能性
がある。
若干の理想的でない面がある。例えば、複雑で内的する
表面に対するフレーム噴霧は困難且つ高価となる可能性
がある。
問題点を解決するための手段
本発明によれば、CrA1M2の粒子を包含する金属マ
トリックスM 〈ここにMlはNiもしくはCoまたは
その両者、M2はy、si、T;、Hf、 Taまたは
希土類元素の内−つ以上〉の複合の電解または無電解析
出により保護層を形成し、保FillのCrAiM2の
粒子より大きい粒度の粒子を包含する金属マトリックス
の複合の電解または無電解析出により固着被覆を形成し
、次いでプラズマ析出プロセスにより耐火物から成る熱
障壁を噴霧コーティングすることにより、支持体上のオ
ーバレイ・コーティングが得られる。
トリックスM 〈ここにMlはNiもしくはCoまたは
その両者、M2はy、si、T;、Hf、 Taまたは
希土類元素の内−つ以上〉の複合の電解または無電解析
出により保護層を形成し、保FillのCrAiM2の
粒子より大きい粒度の粒子を包含する金属マトリックス
の複合の電解または無電解析出により固着被覆を形成し
、次いでプラズマ析出プロセスにより耐火物から成る熱
障壁を噴霧コーティングすることにより、支持体上のオ
ーバレイ・コーティングが得られる。
従って本発明は、保護層と固着被覆とが何れも、フレー
ム噴霧されるのではなく、めっきされる、という点にお
いて、さきに提案されたそれとは異なるものである。
ム噴霧されるのではなく、めっきされる、という点にお
いて、さきに提案されたそれとは異なるものである。
めっきによるM CrAIM2層の生成は、あす
る段階で熱処理により修正されるコーティングを生成す
ることを目的とするGB−2,167,446−Aに既
に提案されており、その明細書は粒度の綿密な制御がな
されるべきことを強調しており、概括的に提示された粒
度の要件は、析出されたコーティング内の粒子の少なく
とも99(重量)%が25μm未満または少なくとも9
5%が3.0〜13.6μ卯である、としている。同明
細書には電着により極めて望ましい表面仕上がりを有す
るコーティングが生成される、と述べである。めっきは
、滑らかな、光沢さえある、表面を備えたコーティング
を生成することで周知されており、この粒度の粒子の析
出されたマトリックスへの結合によって比較的滑らかな
表面が更にもたらされる。噴霧されたMCr/M!Yコ
ーティングは不適切なことに表面が荒いので、充分な付
着性を以て、熱障壁を、噴霧コーティングされたMCr
AjYコーティングへ直接に付着させることはできない
。粗い粒子を用いて噴霧コーティングされた固着被覆が
必要とされていた。従って、熱障壁の素地を用意する際
、複合めっきは全く無用であろうと考・えられる。しか
し、最も驚いたことには、より大きい粒子を含むめっき
された固着被覆を後続させた、めっきされた M CrAIM2被覆によってib満足な素地が得られ
、その上に、層間に全く充分な付着性を保ちながら、噴
霧コーティングにより熱障壁を付着させ得ることが見い
だされたのである。このように、めっきされた固着層は
、荒い定着面を生成するために用いられるが、これは、
平滑度の一つである普通に容認されるめっきされた被覆
の性質と全く反対の何かである。
ることを目的とするGB−2,167,446−Aに既
に提案されており、その明細書は粒度の綿密な制御がな
されるべきことを強調しており、概括的に提示された粒
度の要件は、析出されたコーティング内の粒子の少なく
とも99(重量)%が25μm未満または少なくとも9
5%が3.0〜13.6μ卯である、としている。同明
細書には電着により極めて望ましい表面仕上がりを有す
るコーティングが生成される、と述べである。めっきは
、滑らかな、光沢さえある、表面を備えたコーティング
を生成することで周知されており、この粒度の粒子の析
出されたマトリックスへの結合によって比較的滑らかな
表面が更にもたらされる。噴霧されたMCr/M!Yコ
ーティングは不適切なことに表面が荒いので、充分な付
着性を以て、熱障壁を、噴霧コーティングされたMCr
AjYコーティングへ直接に付着させることはできない
。粗い粒子を用いて噴霧コーティングされた固着被覆が
必要とされていた。従って、熱障壁の素地を用意する際
、複合めっきは全く無用であろうと考・えられる。しか
し、最も驚いたことには、より大きい粒子を含むめっき
された固着被覆を後続させた、めっきされた M CrAIM2被覆によってib満足な素地が得られ
、その上に、層間に全く充分な付着性を保ちながら、噴
霧コーティングにより熱障壁を付着させ得ることが見い
だされたのである。このように、めっきされた固着層は
、荒い定着面を生成するために用いられるが、これは、
平滑度の一つである普通に容認されるめっきされた被覆
の性質と全く反対の何かである。
固着被覆の好適な構成要素は保護層のそれと同一または
それに類似しているがそれは、固着機能を備えることに
加えて、下履をなす保M層が設けられるためのそれと同
様な作動条件にこの被覆がさらされるためである。
それに類似しているがそれは、固着機能を備えることに
加えて、下履をなす保M層が設けられるためのそれと同
様な作動条件にこの被覆がさらされるためである。
保護層を付着させるための好適な構成要素ならびにその
方法は、前述のGB−2,167,446−Aに記述さ
れたそれらであり、使用され得る装置および方法の更に
詳細については、GB−2゜014.189−Aおよび
US−4,305,792を参照されたい。上記の装置
および方法は、固着被覆を付着させるために使用するこ
とができる。
方法は、前述のGB−2,167,446−Aに記述さ
れたそれらであり、使用され得る装置および方法の更に
詳細については、GB−2゜014.189−Aおよび
US−4,305,792を参照されたい。上記の装置
および方法は、固着被覆を付着させるために使用するこ
とができる。
実施例および作用
本発明は種々の方法で実施できるが、ここで例示のため
、ガス・タービン買上の一つの特定のオーバレイの装置
について説明する。
、ガス・タービン買上の一つの特定のオーバレイの装置
について説明する。
翼は先ず、めっきに適した準備処理を施され、一つの例
ににあっては、それが2分間、シアン化物の洗浄剤に浸
せきされ、水洗がこれに続き、塩化第二鉄エッチ液内で
の30秒間の浸せきによりエツチングされ、水洗がこれ
に続き、1dm2当たり3.5Aの電流密度で3分間、
ニッケル浴゛に置くことによりニッケル・ストライクを
施される。
ににあっては、それが2分間、シアン化物の洗浄剤に浸
せきされ、水洗がこれに続き、塩化第二鉄エッチ液内で
の30秒間の浸せきによりエツチングされ、水洗がこれ
に続き、1dm2当たり3.5Aの電流密度で3分間、
ニッケル浴゛に置くことによりニッケル・ストライクを
施される。
次いで翼は、GB−2,014,189−8に記述され
ためつき用バレル内に保持され、陰極接点に接続される
。GB−2,014,189−Bに記述された技法を用
いて0.076〜0.127閲の厚さにCoN1CrA
IYのコーティングが舅に施されるが、バスはCON
iめっき液を包含し、粒子は重1rcr60SAi40
.Y1.7の割合のものを含むCrAj!Yである。粒
度分布は、5μm未満で5(重量)%、10μm未満で
10〜15(重量)%、20μm未満で35〜55(重
量)%の最大値である。別の粒度分布は、5μ而未満で
7.7(重量)%、10μmで56(重量)%、20μ
m未満で94(重量)%、30μm未満で99(重量)
%の最大値である。
ためつき用バレル内に保持され、陰極接点に接続される
。GB−2,014,189−Bに記述された技法を用
いて0.076〜0.127閲の厚さにCoN1CrA
IYのコーティングが舅に施されるが、バスはCON
iめっき液を包含し、粒子は重1rcr60SAi40
.Y1.7の割合のものを含むCrAj!Yである。粒
度分布は、5μm未満で5(重量)%、10μm未満で
10〜15(重量)%、20μm未満で35〜55(重
量)%の最大値である。別の粒度分布は、5μ而未満で
7.7(重量)%、10μmで56(重量)%、20μ
m未満で94(重量)%、30μm未満で99(重量)
%の最大値である。
保護層を備える舅は装置から取り外されて洗浄され、次
いで、同様のコバルトめっき液を包含し且つ保護層のた
めに用いたと同じ組成を有しながら後段に述べるような
異なる粒度分布を有するCrAj!Y粒子を装置に装入
した、英国特許出願第2182055号に記述された装
置内に定置される。最初のM、CrAxY被覆から第二
の定着被覆プロセス段階への移動に遅延が生ずると、構
成要素の表面は、塩化第二鉄エッチ液内での浸せきと最
初の前処理と同様なニッケル・ストライクとにより再活
性化される可能性がある。粒度分布は、150μ乳を超
える粒度については粉末の1%以下、38μm未満の粒
度については15%以下となるようになされる。めっき
は、0.025〜0.15Mの厚さを有する固着被覆を
生成するように行われる。
いで、同様のコバルトめっき液を包含し且つ保護層のた
めに用いたと同じ組成を有しながら後段に述べるような
異なる粒度分布を有するCrAj!Y粒子を装置に装入
した、英国特許出願第2182055号に記述された装
置内に定置される。最初のM、CrAxY被覆から第二
の定着被覆プロセス段階への移動に遅延が生ずると、構
成要素の表面は、塩化第二鉄エッチ液内での浸せきと最
初の前処理と同様なニッケル・ストライクとにより再活
性化される可能性がある。粒度分布は、150μ乳を超
える粒度については粉末の1%以下、38μm未満の粒
度については15%以下となるようになされる。めっき
は、0.025〜0.15Mの厚さを有する固着被覆を
生成するように行われる。
次いで、翼は取り外され、洗浄される。コーティングは
次いで、残余の析出物への表面の粉末の接着を行うため
、真空熱処理される。例えば翼を、1115℃で2時間
、もしくは1050〜1100℃の範囲内で2時間、ま
たは900〜1200℃の範囲内で、1200℃で最大
2時間もしくは900℃で最小1/4時間で、処理する
こともできる。次いで熱障壁が、プラズマ・フレーム析
出プロセスにより、固着被覆上に噴霧される。゛この被
覆は本質的に、重量で、7〜9%のY2O3、最大1.
5%のSi0 .0.5%のCaO10,3%のMob
、0.4%のFe2O3,0,2%のAl2O3および
0.2%のrho、、、それに残余がZrO2という化
学組成を有する8%イツトリア・スタビライズド・ジル
コニアから成る。粒度分布は、74μmを超える粒度に
ついでは最大10%、44μm超については65〜10
0%、44μm未満については最大25%となるように
なされる。真空熱処理を固着被覆の付着後に行う代りに
、それを熱障壁の付着後に同じ方法で行っても良い。
次いで、残余の析出物への表面の粉末の接着を行うため
、真空熱処理される。例えば翼を、1115℃で2時間
、もしくは1050〜1100℃の範囲内で2時間、ま
たは900〜1200℃の範囲内で、1200℃で最大
2時間もしくは900℃で最小1/4時間で、処理する
こともできる。次いで熱障壁が、プラズマ・フレーム析
出プロセスにより、固着被覆上に噴霧される。゛この被
覆は本質的に、重量で、7〜9%のY2O3、最大1.
5%のSi0 .0.5%のCaO10,3%のMob
、0.4%のFe2O3,0,2%のAl2O3および
0.2%のrho、、、それに残余がZrO2という化
学組成を有する8%イツトリア・スタビライズド・ジル
コニアから成る。粒度分布は、74μmを超える粒度に
ついでは最大10%、44μm超については65〜10
0%、44μm未満については最大25%となるように
なされる。真空熱処理を固着被覆の付着後に行う代りに
、それを熱障壁の付着後に同じ方法で行っても良い。
GB−2,014,189−8に記述された方法に代わ
る方法として、本出願人等の英国特許出願第85265
46号(公告第2182055号)に記載の装置および
方法により保護層と固着被膜とを付着させることもでき
る。
る方法として、本出願人等の英国特許出願第85265
46号(公告第2182055号)に記載の装置および
方法により保護層と固着被膜とを付着させることもでき
る。
本発明による上述の方法で片側にコーティングされ、ま
た表面温度を2分間に1050℃に上昇させ且つ2分間
に下降させるためフレームの内外に動かされた、パドル
形試験片についての熱サイクル試験中、この試験片は、
代表的な商業上の容認レベルが500熱サイクルである
ところを、1000熱サイクルに充分に耐えたのである
。
た表面温度を2分間に1050℃に上昇させ且つ2分間
に下降させるためフレームの内外に動かされた、パドル
形試験片についての熱サイクル試験中、この試験片は、
代表的な商業上の容認レベルが500熱サイクルである
ところを、1000熱サイクルに充分に耐えたのである
。
Claims (4)
- (1)支持体上にオーバレイ・コーティングを生成する
方法にして、 1)CrAlM_2の粒子を包含する金属マトリックス
M_1(ここにM_1はNiもしくはCoまたはその両
者、M_2はY、Si、Ti、Hf、Taまたは希土類
元素の内一つ以上)の複合の電解または無電解析出によ
り保護層を形成する段階と、 2)保護層のCrAlM_2の粒子より大きい粒度の粒
子を包含する金属マトリックスの複合の電解または無電
解析出により固着被覆を形成する段階と、 3)プラズマ析出プロセスにより耐火物から成る熱陣壁
を噴霧コーティングする段階とを含む方法。 - (2)特許請求の範囲第1項に記載の方法において、固
着被覆が、保護層の粒子より大きい粒度でありながら、
それと同じ組成であるようにした方法。 - (3)特許請求の範囲1項または第2項に記載の方法に
おいて、保護層の粒子の粒度分布が、5μm未満で5(
重量)%、10μm未満で10〜15(重量)%、20
μm未満で35〜55(重量)%の最大値を有するよう
にした方法。 - (4)特許請求の範囲第3項に記載の方法において、固
着被覆の粒子の粒度分布が、150μm超で1(重量)
%の最大値と、38μm未満で15(重量)%の最大値
とを有するようにした方法。