JPH089499B2 - 焼成マグネシア・ドロマイトれんが - Google Patents

焼成マグネシア・ドロマイトれんが

Info

Publication number
JPH089499B2
JPH089499B2 JP4336706A JP33670692A JPH089499B2 JP H089499 B2 JPH089499 B2 JP H089499B2 JP 4336706 A JP4336706 A JP 4336706A JP 33670692 A JP33670692 A JP 33670692A JP H089499 B2 JPH089499 B2 JP H089499B2
Authority
JP
Japan
Prior art keywords
slag
fired magnesia
magnesia dolomite
dolomite brick
dolomite
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP4336706A
Other languages
English (en)
Other versions
JPH06157131A (ja
Inventor
本 英 司 川
田 毅 吉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
TYK Corp
Original Assignee
TYK Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by TYK Corp filed Critical TYK Corp
Priority to JP4336706A priority Critical patent/JPH089499B2/ja
Publication of JPH06157131A publication Critical patent/JPH06157131A/ja
Publication of JPH089499B2 publication Critical patent/JPH089499B2/ja
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Description

【発明の詳細な説明】
【0001】
【産業上の利用分野】本発明は焼成マグネシア・ドロマ
イトれんがに関するものである。
【0002】
【従来の技術】焼成マグネシア・ドロマイトれんがは主
にAOD炉,溶鋼鍋、VOD鍋等に使用されている。一
般的にマグネシア・ドロマイトれんがの特徴は以下の様
である。
【0003】高塩基度スラグに対する浸蝕性に強い。 比較的スポーリング性に良い。 熱間強度が低く摩耗に弱い。 消化する。 低価格である。
【0004】そして実際に使用すると、低〜中塩基度ス
ラグとの化学的反応,構造スポーリング,あるいは目地
溶損現象がその殆どを占めている。これらの要因は殆ど
はスラグの浸透に起因するものであり、このスラグ浸透
抑制が大きな課題であった。それに対し、マトリック
ス部へのCaO分散 れんがの緻密化 等の策が成されたが、各々消化の問題,スポーリングの
問題により充分満足されるマグネシア・ドロマイトれん
は存在していないのが現状である。
【0005】
【発明が解決しようとする課題】本発明は従来の技術で
は解決されてない耐スラグ浸透性を改善し、それにより
構造スポール性,目地溶損性,摩耗性を大巾に改善する
ことがねらいである。
【0006】
【課題を解決するための手段】本発明ではMgO,Ca
O以外の成分を故意的に添加し、マトリックス部を改善
する手法を採用した。添加物としては種々研究の結果C
23成分が有効であることが判った。Cr23成分は
10μm以下の微粉として添加した。その理由として
少量添加でより分散させるため、マトリックス部に添
加し、結合あるいはスラグ浸透防止といった効果をより
引き出すため、以上を加味すると10μm以下の微粉と
なり、2〜5μmが望ましいと考えられる。
【0007】尚、添加量については種々の配合試験の結
果0.3〜5.0重量%範囲において有効であることが
判った。(表1)これは5.0重量%以上添加すると低
融点鉱物のCaO・CrO3が過剰に生成するためれん
がの製造上、軟化等により問題が生じる、又0.3重量
%以下では効果が小さいことによる。
【0008】
【表1】
【0009】
【作用】Cr23は融液中に混入すると融液の粘性を上
げるため、特にスラグ中のSiO2成分の多い低塩基度
スラグの場合は耐火物中のCr23が、粒界に浸入した
スラグによって生じた融液の粘性を上げ、浸食の進行を
防ぐ効果が大きい。又、高塩基度スラグにおいては、低
酸素分圧下でスラグ中のCaO成分と高融点化合物を形
成する。結果として低塩基度から高塩基度に至るスラグ
の浸透を充分に抑え、高耐蝕性を得ることができる。C
23成分を微粉としてマトリックス部に添加すると、
上記の効果以外に緻密化,強度増加にもつながり、かつ
ドロマイトクリンカーの表面でCaO・CrO3として
CaOを安定させるため耐消化性においても改善される
傾向を示した。
【0010】
【実施例】表1に本発明の実施例と比較例の配合組成と
耐火物の特性を示す。いずれもフェノール系樹脂をバイ
ンダーとして加え、混練,成形,焼成によりれんがを製
作した。本発明品NO.3,4,5は従来品,NO.
1,2,6に比較して耐スラグ浸透性に優れ、それに起
因する耐構造スポーリング性,耐蝕性にも大きな効果が
現われた。
【0011】本発明による実施例NO.4のれんがを5
0тVOD取鍋内張りとして使用した結果表2の様であ
った。
【0012】
【表2】
【0013】従来品は残厚が少なく、非稼動面まで全面
にスラグが浸透していた。又、稼動面は本発明品は従来
品に比べ滑らかでスポーリングの傾向は無かった。
【0014】
【発明の効果】マグネシアとドロマイトを主成分とする
耐火材料に酸化クロム微粉を0.3〜5.0重量%添加
した焼成マグネシア・ドロマイトれんがは実使用におい
てもスラグ浸透厚みで17%減少し、その結果として3
7%の溶損速度の低減が認められ耐スラグ浸透性に大き
な改善効果を得ることができた。またそれにより耐構造
スポーリング性,耐蝕性などにも大きな効果が得られ
た。

Claims (1)

    【特許請求の範囲】
  1. マグネシアとドロマイトを主成分とする耐火材料100
    重量%に対し10μm以下の酸化クロム微粉を0.3〜
    5.0重量%添加してなる焼成マグネシア・ドロマイト
    れんが。
JP4336706A 1992-11-24 1992-11-24 焼成マグネシア・ドロマイトれんが Expired - Lifetime JPH089499B2 (ja)