JPH11273665A - 非水電解液電池およびその製造方法 - Google Patents
非水電解液電池およびその製造方法Info
- Publication number
- JPH11273665A JPH11273665A JP10079596A JP7959698A JPH11273665A JP H11273665 A JPH11273665 A JP H11273665A JP 10079596 A JP10079596 A JP 10079596A JP 7959698 A JP7959698 A JP 7959698A JP H11273665 A JPH11273665 A JP H11273665A
- Authority
- JP
- Japan
- Prior art keywords
- binder
- positive electrode
- electrolyte battery
- electrode
- heat treatment
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
電容量が増大した電極を得られるようにする。 【解決手段】 正極活物質としての二酸化マンガンに、
導電剤としてのアセチレンブラックと、第1の結着剤と
してのPTFEの水性ディスパージョンを添加するとと
もに、第2の結着剤としてのPETの水性ディスパージ
ョンを添加し、これらに適量の水を加えて混合・混練し
て、粘土状の正極合剤を作製する。この正極合剤を空気
中で120℃の温度で乾燥した後、粉砕し、金型に入れ
て圧縮成形して正極ペレット10を作製する。そして、
真空中で200℃の温度で2時間の加熱処理を行った正
極ペレット10を正極缶11内に載置し、正極ペレット
10上に電解液を含浸させたセパレータ12を配置す
る。リチウム負極板13をその内面に圧着した負極キャ
ップ14をガスケット15を介して正極缶11内に圧入
し、正極缶11開口部をかしめ付けて電池を作製する。
Description
池、リチウム二次電池、リチウムイオン蓄電池などのリ
チウム、リチウム合金、リチウムを吸蔵・放出可能な物
質を負極活物質とし、電解液の溶媒として非水溶媒を用
いる非水電解液電池に係り、特に、少なくとも一方の電
極の活物質に結着剤を添加する非水電解液電池およびそ
の製造方法に関するものである。
電池、リチウムイオン蓄電池などのリチウム、リチウム
合金、リチウムを吸蔵・放出可能な物質を負極活物質と
して用い、電解液の溶媒として非水溶媒を用いる非水電
解液電池では、その正極あるいは負極は、活物質粉体と
導電剤などの添加剤を樹脂結着剤を用いて成形するよう
にしている。この場合、電池の組立前に電極内の水分を
除去するための熱処理を行う必要がある。これは電極内
に水分が残留していると、電池内のリチウムが水分と反
応して、電池の内部抵抗が上昇したり、ガスが発生する
などの不具合を生ずるためである。
電極を成形するために用いられる結着剤は、水分除去の
ための熱処理に対する耐熱性と、化学的な安定性との観
点から、フッ素系樹脂が用いられることが一般的であ
る。その中でも、ポリテトラフルオロエチレン(PTF
E)あるいはテトラフルオロエチレン・ヘキサフルオロ
プロピレン共重合体(FEP)が特によく用いられてい
る。
電極において、電極活物質などを成形して実用上十分な
強度を得るためには、通常は電極重量の数%の重量の結
着剤を配合する必要がある。しかしながら、電極の機械
的強度を上げるために結着剤を多く配合すると、その
分、活物質量が相対的に減少し、あるいは、活物質表面
が結着剤で覆われて活物質の利用率が低下するため、電
極の放電容量が減少するという問題点があった。
こで、本発明では、少量の結着剤を用いて、強度が大き
く、かつ放電容量が増大した電極を得ることを目的とし
てなされたものである。このため、本発明の非水電解液
電池は、結着剤として、せん断応力により繊維化する第
1の結着剤と、せん断応力により繊維化しない第2の結
着剤とを用い、第1の結着剤の融点以下で、かつ第2の
結着剤の軟化温度以上で熱処理した電極を備えるように
している。第1の結着剤はせん断応力により繊維化して
結着力を発揮し、第2の結着剤は軟化温度以上の熱処理
で結着力を発揮する。このため、2種類の結着剤の相乗
効果により、少量の結着剤で十分な機械的強度を有する
電極が得られるため、電池容量が増大した非水電解液電
池が得られる。
においては、せん断応力により繊維化する第1の結着剤
と、せん断応力により繊維化しない第2の結着剤とを正
・負極の少なくとも一方の活物質に添加する結着剤添加
工程と、この結着剤添加工程により第1と第2の結着剤
が添加された活物質にせん断応力を付与するようにして
混合する活物質混合工程と、第1の結着剤の融点以下
で、かつ第2の結着剤の軟化温度以上で熱処理する熱処
理工程とを備えるようにしている。
るため、活物質混合工程における混合により、せん断応
力が付与されるようになって結着力を発揮するようにな
るとともに、熱処理工程においてはこの第1の結着剤の
融点以下の温度で加熱されるため、この熱処理により何
ら悪影響が及ぼされない。一方、第2の結着剤はせん断
応力により繊維化しないため、活物質混合工程でせん断
応力を付与されても結着力を発揮するようなことはない
が、熱処理工程においてはこの第2の結着剤の軟化温度
以上で加熱されるため、結着力を発揮するようになる。
2の2種類の結着剤を用い、第1の結着剤は物理的摩擦
力によって繊維化して結着力を発揮した後、第2の結着
剤は熱処理により溶融結合することによって、さらに大
きな結着力を発揮するようになる。この結果、少量の結
着剤を用いても十分な機械的強度を有する電極が得られ
るようになるため、電池容量が増大した非水電解液電池
が得られるようになる。
ルオロエチレン(PTFE)あるいはテトラフルオロエ
チレン・ヘキサフルオロプロピレン共重合体(FEP)
などのフッ素樹脂を用い、第2の結着剤としてポリエチ
レンテレフタレート樹脂(PET)を用いるようにする
と、第1の結着剤として用いたPTFEあるいはFEP
の融点以下、第2の結着剤のPET樹脂の軟化温度以上
で熱処理することにより、電極中でPET樹脂の粒子が
互いに溶融結合し、少ない配合量でも大きな結着強度が
得られる。これにより、結着剤の配合比を減少させるこ
とが可能となるので、活物質粒子の表面を覆う結着剤の
量も低下することとなって、単純な結着剤の添加量減少
効果以上の放電容量の増加が期待できるようになる。
いて電極を成形した場合、十分な電極強度を得ることが
できない。これは、フッ素樹脂とPET樹脂の結着機構
の違いによるものと思われる。すなわち、PTFE、F
EPなどのフッ素樹脂は、せん断応力によって容易に繊
維化するため、成形時に活物質粒子にこの繊維化したフ
ッ素樹脂が絡み合って結着力が得られるようになる。し
かしながら、PET樹脂は繊維化しないため、PET樹
脂粒子のみを活物質と混合してもほとんど結着力を発生
しないため、全く電極の形状に成形することができな
い。このため、これを熱処理して結着力を上げるという
熱処理工程に移行させることが不可能になる。
ルオロエチレンを用いた場合の熱処理温度は170〜3
27℃の範囲とすることが好ましく、第1の結着剤とし
てテトラフルオロエチレン・ヘキサフルオロプロピレン
共重合体を用いた場合の熱処理温度は170〜270℃
の範囲とすることが好ましい。
してのアセチレンブラック5gと、第1の結着剤として
のポリテトラフルオロエチレン(PTFE)の水性ディ
スパージョンをPTFE固形分で1g相当量を添加する
とともに、第2の結着剤としてのポリエチレンテレフタ
レート樹脂(PET)の水性ディスパージョンをPET
固形分で1g相当量を添加し、これらに適量の水を加え
て混合・混練して、粘土状の正極合剤の塊を作製する。
この正極合剤を空気中で120℃の温度で乾燥した後、
粉砕し、金型に入れて圧縮成形して実施例1の正極ペレ
ットaを作製する。正極ペレットaの寸法は直径16m
mで、厚み0.5mmとした。
パージョンの代わりに、テトラフルオロエチレン・ヘキ
サフルオロプロピレン共重合体(FEP)の水性ディス
パージョンをFEP樹脂固形分で1g相当量を用いたこ
とを除いては、実施例1と同様にして正極ペレットを作
製して、実施例2の正極ペレットbとする。
ージョンを用いないことを除いては、実施例1と同様に
して正極ペレットを作製して、比較例1の正極ペレット
cとする。
パージョンを、PTFE樹脂固形分で2g相当量を添加
し、第2の結着剤としてのPETの水性ディスパージョ
ンを用いないことを除いては、実施例1と同様にして正
極ペレットを作製して、比較例2の正極ペレットdとす
る。
パージョンを、PTFE樹脂固形分で5g相当量を添加
し、第2の結着剤としてPETの水性ディスパージョン
を用いないことを除いては、実施例1と同様にして正極
ペレットを作製して、比較例3の正極ペレットeとす
る。
パージョンの代わりにFEPの水性ディスパージョン
を、FEP樹脂固形分で2g相当量を添加し、第2の結
着剤としてのPETの水性ディスパージョンを用いない
ことを除いては、実施例1と同様にして正極ペレットを
作製して、比較例4の正極ペレットfとする。
パージョンの代わりにFEPの水性ディスパージョン
を、FEP樹脂固形分で5g相当量を添加し、第2の結
着剤としてのPETの水性ディスパージョンを用いない
ことを除いては、実施例1と同様にして正極ペレットを
作製して、比較例5の正極ペレットgとする。
パージョンを用いず、第2の結着剤としてのPETの水
性ディスパージョンのみをPET樹脂固形分で5g相当
量を添加したことを除いては実施例1と同様にしたが、
正極ペレットを成形することができなった。従って、こ
の正極合剤を比較例6の正極hとする。
を、図1に示すような、治具20の上に載置し、治具2
0の上に載置された各正極ペレット10に押し棒30を
押し当て、押し棒30で押す力を徐々に強くしていっ
て、各正極ペレット10が割れるときの押圧力を各正極
ペレット10の強度として測定した。なお、強度測定に
際しては、各正極ペレット10を熱処理を行わないで測
定した場合と、各正極ペレット10を真空中で200℃
の温度で2時間の熱処理を行った後に測定した場合の2
種類の測定を行った。
ット10を用い、真空中で200℃の温度で2時間の熱
処理を行った各正極ペレット10を用いて試作電池を作
製する。この試作電池は、図2に示すように、正極缶1
1内に正極ペレット10を載置し、この正極ペレット1
0上に電解液を含浸させたプロピレン製不織布からなる
セパレータ12を配置する。なお、電解液としては、非
水溶媒としてのプロピレンカーボネイト(PC)とジメ
トキシエタン(DME)の1:1混合溶媒に、電解質と
してのトリフルオロメタンスルホン酸リチウム(LiC
F3SO3)を1モル/リットルの濃度で溶解させたもの
を用いる。
6mmの円板状に打ち抜いたリチウム負極板13をその
内面に圧着した負極キャップ14を用意し、負極キャッ
プ14をポリプロピレン製ガスケット15を介して正極
缶11内に圧入し、正極缶11開口部を負極キャップ1
4側にかしめ付けて、コイン型リチウム電池を作製す
る。作製した電池の直径は20mmであり、厚みは1.
6mmである。このようにして作製した電池を2mAの
定電流で放電し、放電終止電圧2.0Vまでの時間から
放電容量を算出した。
および上述のように算出した放電容量を示すと、下記の
表1に示すような結果となった。
よび第2の結着剤は正極合剤の全重量に対する添加量
(重量%)を表している。
樹脂を第2の結着剤に用いた正極ペレットa(実施例
1)および正極ペレットb(実施例2)は熱処理後に正
極ペレット10の強度が大きく増加していることであ
る。これはPET樹脂の軟化温度が170℃であるた
め、200℃の温度での熱処理により、正極ペレット1
0内のPET樹脂粒子が互いに溶融結合し、正極ペレッ
ト10の強度が増すためであると考えられる。
ペレット10は、正極合剤の全重量に対して両結着剤の
合計で2重量%を添加することにより、140〜150
gという大きな強度を得ることができる。また、その放
電容量も90mAhと大きい放電容量の電池が得られ
る。
用いない正極ペレットc(比較例1)、正極ペレットd
(比較例2)、正極ペレットe(比較例3)、正極ペレ
ットf(比較例4)、正極ペレットg(比較例5)にあ
っては、熱処理を行った後であっても正極ペレット10
の強度に変化は見られない。これは、PTFEの融点が
327℃、FEPの融点が270℃であるため、200
℃の熱処理では結着剤に変化が起こらないためである。
脂を用いず、第1の結着剤としてのPTFEあるいはF
EPのみを用いた比較例1〜比較例5では、正極合剤の
全重量に対して1重量%〜2重量%という少量の結着剤
を用いた正極ペレットc(比較例1)、正極ペレットd
(比較例2)および正極ペレットf(比較例4)におい
ては、正極の強度が30g〜60gと小さくなる。一
方、正極合剤の全重量に対して5重量%という多量の結
着剤を添加した正極ペレットe(比較例3)および正極
ペレットg(比較例5)においては、正極強度は140
g〜150gと実施例1,2と同等になるが、その放電
容量は80mAhと実施例1,2より1割以上低下して
いる。
量に対して5%重量と多くした場合の放電容量の低下
が、この量の結着剤の添加により正極活物質量が相対的
に少なくなる量よりもさらに小さくなっている。この理
由は定かではないが、結着剤の添加量が多くなると、そ
の表面が結着剤で覆われる活物質量が多くなり、活物質
の有効表面積が低下することに起因して、添加量以上に
放電容量が低下するものと考えられる。
いて正極ペレット10を作製しようと試みたが、PET
樹脂のみではペレットの成形ができなかった。これは、
PET樹脂粒子はフッ素樹脂粒子のような混合・混練時
のせん断応力による繊維化がおこりにくいため、粒子の
状態のままで存在することとなって、PTFEあるいは
FEPなどのフッ素樹脂のように、繊維化した微粒子の
絡み合いによる結着がおこらないためであると考えられ
る。
1,2で示したように、第1の結着剤としてのPTFE
あるいはFEPと、第2の結着剤としてのPETとを組
み合わせて用いることにより、少ない結着剤の添加量で
大きな正極強度を得ることができるので、相対的に活物
質量を多くできるようになる。また、結着剤の添加量が
少ないため、正極活物質の表面が結着剤で覆われる比率
も小さくなるので、大きな電池容量を得ることができ
る。
明の第1と第2の結着剤を添加するに際して、正極のみ
に適用する例について説明したが、負極として活物質粉
体を結着して成形する場合には、本発明を負極に適用し
てもほぼ同等の効果が得られるようになる。
の結着剤の融点以下でかつ、第2の結着剤の軟化点以上
であればよく、第2の結着剤としてPET樹脂を用いる
場合は、第1の結着剤としてPTFEを用いれば170
℃〜327℃の温度範囲が好ましく、第1の結着剤とし
てFEPを用いれば170℃〜270℃の温度範囲が好
ましい。
発明の非水電解液電池としてコイン型の1次電池に適用
する例について説明したが、本発明は、電池の形状につ
いてはコイン型に限らず、円筒型、角形電池にも適用可
能であり、電池の種類については、1次電池、2次電池
ともに適用可能である。
測定する状態を模式的に示す図である。
構成したコイン型電池を示す断面図である。
タ、13…リチウム負極板、14…負極キャップ、15
…ガスケット、20…治具、30…押し棒
Claims (8)
- 【請求項1】 正・負極の少なくとも一方に結着剤を添
加した電極を備えた非水電解液電池であって、 前記結着剤として、せん断応力により繊維化する第1の
結着剤と、せん断応力により繊維化しない第2の結着剤
とを用い、 前記第1の結着剤の融点以下で、かつ前記第2の結着剤
の軟化温度以上で熱処理した電極を備えたことを特徴と
する非水電解液電池。 - 【請求項2】 前記第1の結着剤としてポリテトラフル
オロエチレンあるいはテトラフルオロエチレン・ヘキサ
フルオロプロピレン共重合体を用い、前記第2の結着剤
としてポリエチレンテレフタレート樹脂を用いたことを
特徴とする請求項1に記載の非水電解液電池。 - 【請求項3】 前記第1の結着剤としてポリテトラフル
オロエチレンを用い、かつ170〜327℃の温度で熱
処理した電極を備えたことを特徴とする請求項1に記載
の非水電解液電池。 - 【請求項4】 前記第1の結着剤としてテトラフルオロ
エチレン・ヘキサフルオロプロピレン共重合体を用い、
かつ170〜270℃の温度で熱処理した電極を備えた
ことを特徴とする請求項1に記載の非水電解液電池。 - 【請求項5】 正・負極の少なくとも一方に結着剤を添
加して製造した電極を備えた非水電解液電池の製造方法
であって、 せん断応力により繊維化する第1の結着剤と、せん断応
力により繊維化しない第2の結着剤とを正・負極の少な
くとも一方の活物質に添加する結着剤添加工程と、 前記第1と第2の結着剤が添加された前記活物質にせん
断応力を付与するようにして混合する活物質混合工程
と、 前記第1の結着剤の融点以下で、かつ前記第2の結着剤
の軟化温度以上で熱処理する熱処理工程とを備えたこと
を特徴とする非水電解液電池の製造方法。 - 【請求項6】 前記第1の結着剤としてポリテトラフル
オロエチレンあるいはテトラフルオロエチレン・ヘキサ
フルオロプロピレン共重合体を用い、前記第2の結着剤
としてポリエチレンテレフタレート樹脂を用いたことを
特徴とする請求項5に記載の非水電解液電池の製造方
法。 - 【請求項7】 前記第1の結着剤としてポリテトラフル
オロエチレンを用いた場合、前記熱処理工程において1
70〜327℃の温度で熱処理するようにしたことを特
徴とする請求項5に記載の非水電解液電池の製造方法。 - 【請求項8】 前記第1の結着剤としてテトラフルオロ
エチレン・ヘキサフルオロプロピレン共重合体を用いた
場合、前記熱処理工程において170〜270℃の温度
で熱処理するようにしたことを特徴とする請求項5に記
載の非水電解液電池の製造方法。