JPS6431996A - 電気メッキ液中の微粒子凝集防止方法 - Google Patents

電気メッキ液中の微粒子凝集防止方法

Info

Publication number
JPS6431996A
JPS6431996A JP18792487A JP18792487A JPS6431996A JP S6431996 A JPS6431996 A JP S6431996A JP 18792487 A JP18792487 A JP 18792487A JP 18792487 A JP18792487 A JP 18792487A JP S6431996 A JPS6431996 A JP S6431996A
Authority
JP
Japan
Prior art keywords
plating
plating bath
fine grains
ultrasonic
plating film
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
JP18792487A
Other languages
English (en)
Inventor
正俊 関口
眞一 鈴木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Steel Corp
Original Assignee
Nippon Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Steel Corp filed Critical Nippon Steel Corp
Priority to JP18792487A priority Critical patent/JPS6431996A/ja
Publication of JPS6431996A publication Critical patent/JPS6431996A/ja
Ceased legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は、電気メッキ液中の微粒子凝集防止方法に関す
るものである。
(従来の技術) 耐腐食性、耐摩耗性を向上させるために、例(丁 え衾、5i02.Af!、203 といったセラミック
微粒子、Crといった金属微粒子、CFnといった炭化
微粒子などを電解メッキ液中に分散させ、Zn、Zn−
Fe。
Zn−Ni、Zn−Cr、Zn−Fe−Ni、Zn−F
e−Go とyuメッキ層中にlnm−1μmの粒径の
微粒子を含有させる複合メッキ方法が公知となっている
。例えば、特開昭61−127900号公報、特開昭[
1l−143597号公報では、SiO2,Aj220
3複合メッキ方法が開示されている。これらのメッキ鋼
板は、例えば自動車等の輸送機関、家電、建材用の防錆
銅板として用いられる。
(発明が解決しようとする問題点) 耐腐食性、耐摩耗性といった性能を安定して得るには、
複合メッキのメッキ層中に含有させる微粒子の粒径を一
定に保たなければならないが、そのためにはメッキ液中
に分散させる微粒子の粒径もまた一定に保つ必要がある
。しかし、これらの微粒子は一般に電解メッキ液中では
ゲル化・沈殿等の凝集を起こし易い。即ち、水溶液中で
は安定なlnm−1μmの微粒子も、メッキ液のような
電解質溶液中では個々の微粒子が集金、@果し、粒径が
巨大化したり、ゲル化・沈殿を生ずることがある。こう
した凝集した微粒子は十分な攪拌を行なっても元の粒径
にはならず、微粒子の粒径が不安定となって、長期的に
安定した組成の複合メッキ鋼板の製造が困難となる。そ
して、この凝集を防止する有効な手段は見つかっていな
い。そこで、本発明は、このような微粒子の凝集を防止
することでメッキ液の安定性を長期的に保つ凝集防止方
法を提供する。
(問題点を解決するための手段) 本発明は、メッキ液中へ微粒子を添加し、メッキ金属と
共析させるに際し、メッキ液中へ超音波を照射すること
を特徴とする電気メッキ液中の微粒子凝集防止方法であ
る。
(作 用) この凝集という現象が起こる理由についてははっきりと
した理論的解明がなされてはいないが、微粒子の水和層
がメッキ液中の電解質により剥奪され、ゲル化・沈殿等
の凝集が起こるものと考えられる。このため、この凝集
を防ぐためには個々の微粒子に十分なエネルギーを与え
ればよい。そこで、メッキ液中の微粒子に与えるエネル
ギー供給方法を種々検討した結果、超音波を照射させる
ことが有効であることを見出した。
例えば、2n、2n−Fe、Zn−Ni、Zn−Cr、
Zn−Fe−Ni、Zn−Fe−C○といったメッキ液
の電解質を含むイオン濃度として0.5〜3 moil
 / Il、 5i02.  AJ1203 といった
セラミック微粒子、Crといった金属微粒子、CFnと
いった炭化微粒子の濃度として1〜400g/fl、ま
た分散させる微粒子の粒径としてlnm−1μmという
メ・メーにおいて、超音波照射による11!防止効果が
見られる。照射させる超音波の周波数は19KHz〜2
 MHzの範囲で)凝集防止に十分な効果がある。19
KHz未満でも効果はあるが、騒音等大きく好ましくな
い。又2 MHz超になると高出力が得られにくく、設
備費も高価になり、好ましくない。
超音波の出力および照射時間は、メッキ液の容量、電解
質イオン濃度、微粒子の濃度、浴温等によって適宜法め
ればよく、また連続的に照射しても断続的に照射しても
効果はある。
照射方法としては、超音波振動子を直接メッキ槽中に浸
漬させる方法、メッキ槽下部に振動子を取り付ける方法
、メッキ槽を水中に浸漬させ、超音波を水中に照射させ
間接的にメッキ液に照射さパイプ等の経路においてメッ
キ液に照射することによっても微粒子の凝集を確実に防
止できる。
第1図から第3図までは、メッキ液へ超音波を照射する
例を示す。1°は超音波発生装置、2は超音波発振子を
示す。第1図は、メッキi& 4中に超音波発振子2を
浸漬させる方法、第2図はメッキ槽3の底部に超音波発
振子2を設置する方法、第3図はメッキ槽3を水槽5中
へ設置し、水6中に浸漬させた超音波発振子2より間接
的に超音波を照射する方法であるが、この際メッキ槽3
の材質は、固体中の音速が水のものに近い例えばガラス
などが適している。
以下実施例にもとづいて本発明の内容をさらに詳しく説
明する。
(実施例) Zn−Feメッキに5t(h微粒子を含有させる複合メ
ッキ製造を例にとり、本発明による凝集防止を実施した
。第1表の組成をもつメッキ液に第1図に示す方法で超
音波を照射させた。周波数は!9.5Kllz、出力2
00W、照射方法は第2表に示すとおりである。これら
のメッキ液(50℃)を用いて、冷延鋼板にメッキ(重
流密度150 A/dm’、付若二20 g/m勺を施
し、メッキ外観および微粒子の含有について評価した。
第3表に示すとおり、超音波を照射させないメッキ液で
複合メッキを行なうと、メッキ液調整後4日目でメッキ
外観不良および微粒子がメッキ層中に含有しない現象が
起こった。しかし、超音波を照射させたメッキ液では、
調整後30日経過しても外観良好でかつ微粒子をメッキ
層中に含有させることができた。
ちなみに、メッキ液中に分散させた5i02微粒子の粒
径を測定したところ、メッキ液調整直後で平均粒径11
00nであったものが、30日経過後で、超音波を照射
しないものが10μmになっていた。しかし超音波を照
射したメッキ液は30日経過後でも、90nm〜120
nmといずれも粒径の安定性が保たれていた。
又周波数を28KHz 、  50KHzと変化して実
施したところ同様に好結果が得られた。
第  2  表 第   3   表 上段二表面外観 下段:微粒子の含有状態(発明の効果
) 本発明により、電解メッキ液中に分散させた微粒子の凝
集を抑制でき、長期的に安定な複合メツ果が得られる。
【図面の簡単な説明】
第1図〜第3図は超音波照射方法の例を示す図である。 1・・・超音波発生装置、2・・・超音波光・振子、3
・・・メッキ槽、4・・・メッキ液、5・・・水槽、6
・・・水。 代理人 弁理士  秋 沢 政 光 他  1  名 左I図 つ 第3図 /−起音j皮梵生装置 2−感音j皮発赤今 4−−−メ゛ソ矢jギと

Claims (1)

    【特許請求の範囲】
  1. (1)メッキ液中へ微粒子を添加し、メッキ金属と共析
    させるに際し、メッキ液中へ超音波を照射することを特
    徴とする電気メッキ液中の微粒子凝集防止方法。
JP18792487A 1987-07-28 1987-07-28 電気メッキ液中の微粒子凝集防止方法 Ceased JPS6431996A (ja)