JPS5835544A - 電子写真用感光体 - Google Patents
電子写真用感光体Info
- Publication number
- JPS5835544A JPS5835544A JP13429681A JP13429681A JPS5835544A JP S5835544 A JPS5835544 A JP S5835544A JP 13429681 A JP13429681 A JP 13429681A JP 13429681 A JP13429681 A JP 13429681A JP S5835544 A JPS5835544 A JP S5835544A
- Authority
- JP
- Japan
- Prior art keywords
- protrusions
- support
- depth
- less
- photoreceptor
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
め要約のデータは記録されません。
Description
【発明の詳細な説明】
本発明は電子写真法において用いられる感光体に関し、
詳細には、感光体の支持体の表面粗さを特定値以下にす
ることによって、コピー画質を大いに向上した感光体に
関する。
詳細には、感光体の支持体の表面粗さを特定値以下にす
ることによって、コピー画質を大いに向上した感光体に
関する。
従来よシミ子写真法において、種々の感光体が実用に供
されているが、コピー品質の点からよシ一層の改善が要
求され、各方面から検討されている。
されているが、コピー品質の点からよシ一層の改善が要
求され、各方面から検討されている。
本発明もこの要求に応えるべく研、究されたものでアシ
、特には、感光体支持体の表面状態を種々検討すること
によって最適な条件を見い出そうとして成されたもので
ある。
、特には、感光体支持体の表面状態を種々検討すること
によって最適な条件を見い出そうとして成されたもので
ある。
本発明者らの研究によれば、従来の感光体において用い
られていた導電性支持体の表面には多くの突起が存在し
て凹凸状を成し、感光体用としては表面が粗過ぎ、これ
が原因となり多くの問題を引起していることが判った。
られていた導電性支持体の表面には多くの突起が存在し
て凹凸状を成し、感光体用としては表面が粗過ぎ、これ
が原因となり多くの問題を引起していることが判った。
すなわち、多くの突起を有する凹凸状の支持体表面にS
s又はSe −As + Se −T’s等の光導電層
を形成した場合、これら支持体表面の突起が核となって
更に突起径が60μm以上もの大きな突起に生長し光導
電層膜表面に点在する。このような感光体を複写プロセ
スに用いると帯電ムラや光導電−表面のブロッキング層
破壊が生じ鮮明画像が得られない。更に前記突起は、複
写プロセスでのクリーニング工程においてクリーニング
部材の破損、摩耗を起し、クリーニング不良を招く。
s又はSe −As + Se −T’s等の光導電層
を形成した場合、これら支持体表面の突起が核となって
更に突起径が60μm以上もの大きな突起に生長し光導
電層膜表面に点在する。このような感光体を複写プロセ
スに用いると帯電ムラや光導電−表面のブロッキング層
破壊が生じ鮮明画像が得られない。更に前記突起は、複
写プロセスでのクリーニング工程においてクリーニング
部材の破損、摩耗を起し、クリーニング不良を招く。
この結果コピー画像上にいわゆる黒スジが発生する。
以上の如き知見に基づき種々研究を重ねたところ、導電
性支持体表面において一、R接する突起間隔(以下、突
起ピッチという)を0.50 +u以下とし、且つ突起
の深さく通常これを面粗さということが多い)を0.3
0μmとするようにすると、前述の如き突起による現象
は解決されることが判った。特に、前記突起のピッチが
0.30n以下、゛突起深さ0.10μm以下の場合に
は、導電性゛支持体の表面は極めて平滑であり、光導電
層を蒸着法等で形成した場合にも大きな突起に生長する
ようなことはない。
性支持体表面において一、R接する突起間隔(以下、突
起ピッチという)を0.50 +u以下とし、且つ突起
の深さく通常これを面粗さということが多い)を0.3
0μmとするようにすると、前述の如き突起による現象
は解決されることが判った。特に、前記突起のピッチが
0.30n以下、゛突起深さ0.10μm以下の場合に
は、導電性゛支持体の表面は極めて平滑であり、光導電
層を蒸着法等で形成した場合にも大きな突起に生長する
ようなことはない。
以上の如き表面状態を達成する手段としては、超精密旋
盤で鏡面を形成する方法を用いることが好ましく、特に
該方法と従来よシ公知の洗浄。
盤で鏡面を形成する方法を用いることが好ましく、特に
該方法と従来よシ公知の洗浄。
エツチング等の前処理工程を組合わせて行なうと、表面
は容易に目的とする平滑さとなり且つ表面の汚染物も除
去される。
は容易に目的とする平滑さとなり且つ表面の汚染物も除
去される。
以下、本発明を実施例を挙げて説明する。
実施例
以下の工程に従って、通常旋盤加工仕上シの直径120
fl、長さ400111のAt導電性支持体表面を平滑
化し% AlI2Se3合金の光導電層膜を約60μm
で真空蒸着し、感光体を作成した。
fl、長さ400111のAt導電性支持体表面を平滑
化し% AlI2Se3合金の光導電層膜を約60μm
で真空蒸着し、感光体を作成した。
支持体表面を超精密旋盤(豊田加工機製)によって突起
ピッチ0.10111以下、突起深さ0.05μm以下
とする(ピッチ、深さの測定は、以下も同様に表面粗さ
計を用いた)。次いで支持体をA−クレン洗浄後、Na
3PO43wt%水溶液中で約50秒間アルカリエツチ
ングを施し、水洗を2度繰返し、80℃の湯洗水中に1
分間浸漬、乾燥した。この時の突起ピッチは0.101
111以下、突起深さは0.08μm以下であった。
ピッチ0.10111以下、突起深さ0.05μm以下
とする(ピッチ、深さの測定は、以下も同様に表面粗さ
計を用いた)。次いで支持体をA−クレン洗浄後、Na
3PO43wt%水溶液中で約50秒間アルカリエツチ
ングを施し、水洗を2度繰返し、80℃の湯洗水中に1
分間浸漬、乾燥した。この時の突起ピッチは0.101
111以下、突起深さは0.08μm以下であった。
以上のように表面が平滑にされた゛At導電性支持体を
蒸着装置内にセットし、該支持体を毎分13回転で回転
しながら1、支持体温度200℃、蒸着源温度400℃
、真空度10−5torrの条件でA 112 S e
sを35分間真真空層し本発明による感光体を作成し
た。
蒸着装置内にセットし、該支持体を毎分13回転で回転
しながら1、支持体温度200℃、蒸着源温度400℃
、真空度10−5torrの条件でA 112 S e
sを35分間真真空層し本発明による感光体を作成し
た。
蒸着後の光導電層表面を顕微鏡下で観察したところ、測
定面積約100cIrL当シ、突起径が60μm以上に
生長した突起は2コしか認められず、平滑であった〇 比較例 上記実施例において超精密旋盤加工を超存上げ加工にし
て突起ピッチ約0.51m %突起深さ0.50μmと
する他は同様の処理を施して感光体を作成した。80℃
の湯洗水に浸漬後乾燥した時の突起ピッチ、深さはそれ
ぞれ約Q、 5111 %’ 0.5μmで超仕上げ加
工後の測定値と同様であった。
定面積約100cIrL当シ、突起径が60μm以上に
生長した突起は2コしか認められず、平滑であった〇 比較例 上記実施例において超精密旋盤加工を超存上げ加工にし
て突起ピッチ約0.51m %突起深さ0.50μmと
する他は同様の処理を施して感光体を作成した。80℃
の湯洗水に浸漬後乾燥した時の突起ピッチ、深さはそれ
ぞれ約Q、 5111 %’ 0.5μmで超仕上げ加
工後の測定値と同様であった。
このように作成された比較品について実施ψ1と同様に
して表面観察したところ約100cvL2の測定面積当
りに突起径60μm以上の突起力;70個以上見い出さ
れ表面状態は悪いものであった。
して表面観察したところ約100cvL2の測定面積当
りに突起径60μm以上の突起力;70個以上見い出さ
れ表面状態は悪いものであった。
以上説明したように、本発明は、導電性支持体上に光導
電層を形成するに先立って、支持体表面の粗さを特定値
以下に前処理することによシ光導電層表面をより平滑に
し、特性を向上したものである。
電層を形成するに先立って、支持体表面の粗さを特定値
以下に前処理することによシ光導電層表面をより平滑に
し、特性を向上したものである。
特許出願人 株式会社リコー
代理人弁理士 小 松 秀 岳
228−
Claims (1)
- 導電性支持体表面において)隣接“する突起の間隔が0
.50m以下で、且つ突起の深さが0.30μm以下で
あることを特徴とする電子写真用感光体。